Next Article in Journal
Effects of Mung Bean (Vigna radiata) Protein Isolate on Rheological, Textural, and Structural Properties of Native Corn Starch
Next Article in Special Issue
Carbonized Leather Waste: A Review and Conductivity Outlook
Previous Article in Journal
Innovative Coating–Etching Method of Biocarrier Fabrication for Treating Wastewater with a Low C/N Ratio
Previous Article in Special Issue
Biosorbents Based on Biopolymers from Natural Sources and Food Waste to Retain the Methylene Blue Dye from the Aqueous Medium
 
 
Font Type:
Arial Georgia Verdana
Font Size:
Aa Aa Aa
Line Spacing:
Column Width:
Background:
Article

Optimization of Biocomposite Film Based on Whey Protein Isolate and Nanocrystalline Cellulose from Pineapple Crown Leaf Using Response Surface Methodology

1
Doctoral Program, School of Engineering, Post Graduate Program, Universitas Syiah Kuala, Banda Aceh 23111, Indonesia
2
Department of Chemical Engineering, Universitas Syiah Kuala, Banda Aceh 23111, Indonesia
3
Faculty of Integrated Technologies, Universiti Brunei Darussalam, Bandar Seri Begawan BE1410, Brunei
4
Department of Chemistry, Faculty of Science, Universiti Brunei Darussalam, Jalan Tungku Link, Bandar Seri Begawan BE1410, Brunei
5
Faculty of Food Science and Nutrition, Universiti Malaysia Sabah, Kota Kinabalu 88400, Sabah, Malaysia
*
Authors to whom correspondence should be addressed.
Polymers 2022, 14(15), 3006; https://doi.org/10.3390/polym14153006
Submission received: 14 May 2022 / Revised: 18 July 2022 / Accepted: 21 July 2022 / Published: 25 July 2022

Abstract

:
This study employed response surface methodology to optimize the preparation of biocomposites based on whey protein isolate, glycerol, and nanocrystalline cellulose from pineapple crown leaf. The effects of different concentrations of nanocrystalline cellulose as a filler and glycerol as a plasticizer on the thickness, the tensile strength, and the elongation at break on the resulting biocomposite films were investigated. The central composite design was used to determine the optimum preparation conditions for biocomposite films with optimum properties. The regression of a second-order polynomial model resulted in an optimum composition consisting of 4% glycerol and 3.5% nanocrystalline cellulose concentrations, which showed a desirability of 92.7%. The prediction of the regression model was validated by characterizing the biocomposite film prepared based on the optimum composition, at which the thickness, tensile strength, and elongation at break of the biocomposite film were 0.13 mm, 7.16 MPa, and 39.10%, respectively. This optimum composition can be obtained in range concentrations of glycerol (4–8%) and nanocrystalline cellulose (3–7%). Scanning electron microscope images showed that nanocrystalline cellulose dispersed well in the pure whey protein isolate, and the films had a relatively smooth surface. In comparison, a rough and uneven surface results in more porous biocomposite films. Fourier transform infrared spectroscopy revealed that nanocrystalline cellulose and glycerol showed good compatibility with WPI film by forming hydrogen bonds. The addition of nanocrystalline cellulose as a filler also decreased the transparency, solubility, and water vapor permeability and increased the crystallinity index of the resulting biocomposite film.

1. Introduction

The development of biodegradable materials for food packaging has been significantly increasing due to the various environmental problems associated with synthetic materials derived from petroleum [1]. Biopolymer materials extracted from biomass are generally classified into three groups, polysaccharide, protein, and lipid, and are the biodegradable materials in focus [2], due mainly to their status as low-cost, renewable, abundant, and easily accessible [3]. These materials can also be extracted from agricultural byproducts or waste, increasing their added value and providing significant economic and environmental benefits [4]. Particularly, whey protein isolate (WPI), a valuable by-product of cheese and casein production, consisting of more than 90 wt% protein, is an attractive biopolymer for food packaging applications because of several benefits, such as biodegradability, good film-forming properties, biocompatibility, and abundance in nature [5,6]. Previous studies have been conducted using other proteins as biodegradable materials to develop the packaging film that can be obtained from plant, animal and microbial sources [4,7,8,9]. WPI-based films also provide functional properties, such as transparency, flexibility, and an excellent barrier against oxygen permeation, which are attractive for food packaging applications [10,11,12]. However, the hydrophilic nature of WPI-based films and their low mechanical and high water vapor permeability as biodegradable materials limited their ability to reach broad commercial applications [13,14,15].
Several strategies have been used to improve the properties of WPI-based films, including the incorporation of biomaterials, nanomaterials, plasticizers, and other crosslinking agents to form biocomposite films that incorporate the advantages of biopolymers while minimizing their drawbacks [16,17]. Numerous studies on WPI (protein) based film with the incorporation of nanomaterials such as nanocrystalline cellulose have demonstrated vast improvements on the mechanical properties of the resulting biocomposite films [18,19,20].
Due to its sustainability, availability, lightness, large surface area, and high mechanical strength, nanocrystalline cellulose (NCC) has attracted a great deal of interest as a potential nano-reinforcement for WPI-based films [18,21]. NCC is a nanometer-sized crystal particle produced as a stable aqueous colloidal suspension and is typically isolated from cellulose sources through acid hydrolysis [22]. Isolation of NCC was reported from different sources such as sugarcane baggases [21], rice straw [23], kenaf bast [24], conorcapus fiber [25], walnut shell [26], and pineapple crown leaf [22].
Pineapple is a common fruit which is widely used as a source of food production. The global market for pineapple and its products has shown a significant increase [22]. Annually, pineapple processing generates 3 billion tons of by-products such as pineapple crown leaf, which causes environmental issues [27]. In several cases, pineapple crown leaves are burned or disposed of in landfills with no regard for the environment. Hence, suitable methods for converting pineapple crown leaves to upgraded products must be implemented.
Pineapple crown leaf fibers were identified as an excellent source of cellulose [28]. Pineapple crown leaves contain 79–83% cellulose, 29% hemicellulose, and 5–15% lignin [29]. In our previous study, the use of pineapple crown leaves as the source of nanocrystalline cellulose (NCC) offered interesting properties that can be used in several applications, which was proven by an improvement to the physical and mechanical properties of whey protein film [18]. Due to this advantage, NCC derived from pineapple crown leaf can partially replace the conventional synthesized polymer packaging materials, while achieving environmental standards. Furthermore, adding plasticizers such as glycerol to the biocomposite film can improve the toughness and minimize brittleness while enhancing polymer chain mobility [30]. Zhai et al. recently reported that adding glycerol could enhance the ductility and elasticity of a WPI film [31].
When preparing a biocomposite film, it is critical to determine the optimum concentrations of the casting solution film compositions to achieve the required composite film properties. Central composite design (CCD) using response surface methodology (RSM) is commonly used to attain this objective. RSM is a mathematical and statistical technique that provides optimal conditions by analyzing the relative importance of all influencing factors [32]. Furthermore, the mathematical models generated by RSM can reveal the interactions between the components of a biocomposite film and its properties by fitting mathematical models from the analysis of variance (ANOVA) [33]. Recent studies have used RSM to achieve optimal formulation in biocomposite film properties such as soy protein films with the addition of glycerol [34], corn starch–chitosan films with the addition of starch nanocrystals [35], and zein films with the addition of gelatin and glutaraldehyde [36]. In this study, the optimization of WPI-based film with the addition of glycerol and nanocrystalline cellulose from pineapple crown leaf using RSM was investigated. The objective of this study was to determine the optimization or the best design parameters of WPI-based film with incorporations of different range concentrations of glycerol (4–8%) and NCC (3–7%) from pineapple crown leaf using RSM-CCD and to investigate the physical and mechanical properties of prepared films.

2. Materials and Methods

2.1. Materials

Whey protein isolate containing 90% protein was purchased from Glanbia Nutritionals (Carlsbad, California, United States). Glycerol, sodium hydroxide (NaOH), hydrogen peroxide (H2O2), and sulfuric acid (H2SO4) were obtained from Merck (Darmstadt, Germany). The NCC was prepared from the isolation of pineapple crown leaf waste using the acid hydrolysis method according to the protocol established earlier [22].

2.2. Isolation of Nanocrystalline Cellulose

The pineapple crown leaf (PCL) waste was first washed and dried as illustrated in Figure 1. Pre-chemical treatment and hydrolysis were used to isolate the NCC according to a method reported earlier [22]. Firstly, the dried PCL was ground and sieved under 40 mesh. The ground fibers were treated in 1 M NaOH and 1 M H2O2 at 80 °C for 1 h to perform the alkali and bleaching treatment. The fiber residue from the alkali and bleaching treatments was washed several times with distillate water until it reached a neutral pH. Acid hydrolysis was then carried out using 1 M H2SO4 for 3 h at 45 °C to produce NCC particles through the depolymerization process. The distilled water was added to resulting solution and cooled in a water bath at 20 °C for 24 h to stop the acid hydrolysis. The suspension was neutralized by centrifugation at 2000 rpm for 30 min with repeated additions of distilled water, followed by ultrasonication for 30 min to remove the excess acid. The NCC product was then dried and ground into powder before being stored at room temperature until further use.

2.3. Preparation of Whey Protein/Nanocrystalline Cellulose/Glycerol Biocomposite Films

Biocomposite films were produced via the solution casting method reported earlier by Fitriani et al. [14] with a few minor modifications, as illustrated in Figure 1. To hydrate the proteins, 6% (w/v) WPI solution was prepared in 200 mL distilled water at pH 8 (pH was regulated with NaOH) using a mechanical stirrer for 30 min at room temperature. The WPI solution was then immersed in a 90 °C water bath with constant stirring for 30 min to denaturize the protein. The WPI solution was then mixed with glycerol of varying amounts (4%, 6%, and 8% w/w) and NCC of varying amounts (3%, 5%, and 7% w/w) using a mechanical stirrer at room temperature for 30 min with a speed of 250 rpm. The WPI and WPI/NCC solution films were poured into 20 cm × 15 cm silicon mold and dried by oven drying at 60 °C for 24 h. All biocomposite films were stored at room temperature until analysis.

2.4. Physical and Mechanical Properties

For each film sample, the thickness was measured using a micrometer with a 0.001 mm accuracy at five different random areas. Using the average thickness value, the mechanical parameters of the film sample were calculated. The mechanical characteristics of the biocomposite films were determined using an MTS Exceed Universal Testing Machine E43 (Eden Prairie, MN, USA) according to the ASTM standard method D638 Type IV.

2.5. Morphological, Physical, and Crystallinilty Analysis of Optimized Biocomposite Films

A scanning electron microscope was used to examine the surface and cross-sectional morphology of the biocomposite films (SEM, JEOL JSM-6360OLA, Tokyo, Japan). The films were coated with a thin layer of gold before being observed at 14 kV. A Fourier transform infrared spectrophotometer was used to measure the functional groups of the films (FTIR, IRPrestige-21, Shimadzu, Kyoto, Japan). The spectra of the films were obtained using 25 scans at a resolution of 4 cm1 for each sample, with scanning ranges ranging from 4000 to 400 cm−1. The transparency of the optimized films was analyzed using a UV-Vis spectrophotometer (UV-1700, Shimadzu, Kyoto, Japan) at a wavelength of 300–800 nm according to ASTM D1746-09 standard. The water solubility (WS) of films was measured using the following procedure. Films with dimensions of 3 cm × 3 cm were dried in an oven at 50 °C for 5 h followed by weighing to measure the initial dry weight. The films were then immersed in 40 mL of distilled water for 24 h at room temperature. The final dry weight was obtained after the insoluble films were dried in an oven at 110 °C for 5 h, and the water solubility (WS, %) of the films was then determined according to Equation (1).
WS   ( % ) = Initial   dry   weight     Final   dry   weight Initial   dry   weight   × 100
The water vapor permeability (WVP) of the films was determined using the gravimetric method, followed by a modified procedure of the ASTM E96 standard [37]. The films were sealed in an 8 mm diameter glass permeation cup. Then, the cups were filled with distilled water and placed in a desiccator to achieve 100% air humidity. Over 48 h, the cup was weighed every 3 h. The water vapor permeability (WVP, g/m.s.Pa) was calculated according to Equation (2).
WVP = C × T A × Δ P
where C is the water vapor transmission rate (g/s), T is the thickness of the films (mm), A is the area of exposed film (mm2), and Δ P is the difference in water vapor pressure all over the films (Pa). The crystallinity of the film was analyzed using an X-ray diffraction Shimadzu XDR 7000 (Japan) with CuKα radiation (λ = 0.1541) operating at 40 kV and 30 mA. The 2θ angle was scanned in the range of 10–70°. The crystallinity index (CI, %) was calculated using the Segal method, as given by Equation (3) [38].
CI   ( % ) = I 200   I am I 200   × 100
where I200 is the maximum intensity of the largest crystal plane reflection (2θ = 22°) and Iam is the minimum intensity of the diffraction at 2θ = 9.5°.

2.6. Experimental Design and Statistical Analysis

The formulation for the fabrication and optimization of biocomposite films was designed using RSM based on CCD. Design Expert 11 (Stat-Ease Inc., Minneapolis, MN, USA) was used to create the experiment design. The two independent variables were the glycerol concentrations (X1) and NCC concentrations (X2). Four axial experiments of levels ±α, eight factorial experiments of levels ±1, and four replicates in the center point were included in the design. The level of factors and the code of variables are shown in Table 1.
The design matrix for biocomposite films is shown in Table 2. The response functions for thickness, tensile strength, and elongation at break were evaluated. For each factor of responses, a second-order quadratic model as a function of X was fitted using Equation (4):
Y = β 0 + i = 1 3 β i X i + i = 1 3 β ii X 1 2 + i = 1 3 β ij X i X j
where Y is the predicted response, β0 is the constant, βi represents the coefficients variable for linear terms, βii denotes the coefficients variable for quadratic terms, βij represents the coefficients variable for interactive terms, and X1 and X2 are the independent variables of glycerol and NCC concentrations, respectively. The variation of each factor was classified into three categories, namely linear, quadratic, and interactive. The relevance of these variables and the adequacy of the second-order quadratic function were determined using the components’ lack-of-fit and error.

3. Results and Discussion

3.1. Thickness, Tensile Strength, and Elongation of Biocomposite Films

Table 3 summarizes the results of the 13 conducted experiments used to determine the thickness, tensile strength, and elongation of the biocomposite films prepared based on the optimum composition suggested by RSM. The concentrations of glycerol and NCC were the two tested factors. The thickness of the biocomposite film was found to be in the range from 0.07 to 0.24 mm. The tensile strengths of biocomposite films were 1.64–7.85 MPa., and the elongation at break was 4.71–42.92%. The highest thickness (0.24 mm) was obtained for the biocomposite film containing 8% glycerol and 7% NCC. The highest tensile strength was 7.85 MPa at 3.17% glycerol and 5% NCC. Meanwhile, the highest elongation was at 42.92% at 6% glycerol and 2.17% NCC.
In general, the crystal formation can occur when natural fibers are utilized as the filler materials in biopolymer matrices like NCC, limiting the physical and mechanical properties of the biocomposite films [21,39]. The thickness, tensile strength, and elongation at break of the prepared biocomposite films were analyzed using RSM-CCD, and the impacts of the independent factors on the responses are further discussed below.

3.2. Model Selection and Verification of Thickness, Tensile Strength, and Elongation

To test the significance of the coefficient terms, all the response variables of biocomposite films were analyzed using ANOVA and regression analysis for model fitting. Table 4, Table 5 and Table 6 show the ANOVA for the quadratic model responses for the thickness, the tensile strength, and the elongation at break parameters, respectively.
The ANOVA test revealed that the quadratic regression models of the thickness, the tensile strength, and the elongation at break were highly significant (p < 0.05). This probability value indicates that the F-value was extremely unlikely to occur because of the noise [40]. Meanwhile, the lack of fit test provides information on the adequacy of the fitted model by measuring the error caused by a defect in the model [41]. The findings revealed that the p-values for lack of fit were non-significant (p > 0.05) for all responses, indicating that the model was well-fitting and sufficient for data explanation. The opposite of lack-of-fit of the model for biocomposite films was further investigated using the R2 value. The results showed that R2 of the biocomposite films model for the thickness, the tensile strength, and the elongation at break were 0.9054, 0.9408, and 0.9455, respectively. Additionally, the adequate precision value was significantly greater than 4 for all responses, indicating that all response surface models had acceptable values. Based on those statistical analyses, the developed experimental models are suitable for predicting the physical and mechanical properties of biocomposite films within the experimental limits in this study.
The p-values for each response from biocomposite films are presented in Table 7. It was indicated that the model terms had a significant effect on the variable responses in biocomposite film properties. The glycerol (X1), NCC (X2), interaction of glycerol and NCC (X1X2), two-level interaction of glycerol (X12), and two-level interaction of NCC (X22) were all significant (p < 0.05) for the thickness and tensile strength properties. However, the interaction of glycerol and NCC (X1X2) was not significant for the elongation property, whereas the other model terms were found to be significant. This can occur because a higher regression value directly interprets a more significant impact of the independent variables in biocomposite films on the variable responses of film properties [42].
For all responses, glycerol and NCC gave the highest regression coefficient values. As a result, glycerol and NCC had the most significant impact on the physical and mechanical properties of the biocomposite films. Furthermore, the positive coefficients for the glycerol and NCC variables indicated a significant effect on the properties of the film. The negative coefficients for the two variables, on the other hand, show an excellent dividing effect on the properties of the biocomposite films [41]. The biocomposite films fit the quadratic regression model better for thickness, tensile strength, and elongation at break. Equations (5)–(7) in terms of the coded values represent the estimated models built for the thickness, tensile strength, and elongation at break methods, respectively. However, it should be acknowledged that the following equations are only limited within the range of tested glycerol concentration (4–8%) and NCC concentration (3–7%).
Y 1 = 0 . 2064 + 0 . 0235 X 1 + 0 . 0328 X 2 + 0.0364 XY 0.0430 X 1 2 0.0352 X 2 2
Y 2 = 4.38 1.83 X 1 0.4423 X 2 + 0.9812 XY + 0.2399 X 1 2 0.9858 X 2 2  
Y 3 = 35.41 10.59 X 1 9.21 X 2 + 2.51 XY 7.47 X 1 2 4.50 X 2 2
where Y1, Y2, and Y3 are the predicted response for thickness, tensile strength, and elongation at break, X1 is glycerol concentration, and X2 is NCC concentration. The regression between the model and experimental data were for thickness, tensile strength, and elongation at break indicate that the quadratic model fits are acceptable, with R2 values being 0.9054, 0.9408, and 0.9455, respectively. This value indicated that the models could not explain only 9.46% of the thickness, 5.92% of the tensile strength, and 5.45% elongation at break variation.

3.3. Analysis of Response Surface of Thickness, Tensile Strength, and Elongation

Figure 2 shows the 3D response surface and contour plots of the effect of independent variables of glycerol and NCC concentrations on thickness, tensile strength, and elongation at break using Equations (3)–(5). The 3D response surface was obtained by varying the two variables of glycerol and NCC. It can be clearly seen that the concentrations of glycerol and NCC have a quadratic effect on the physical and mechanical properties of the biocomposite films. Figure 2a demonstrates that the concentration of glycerol and NCC has a significant effect on thickness. When glycerol concentration rises from 4% to 6% and NCC concentration rises from 3% to 5%, the thickness increased in a parabolic trend. Furthermore, increasing the NCC and glycerol concentrations resulted in thicker biocomposite films. The maximum thickness of 0.24 mm was observed at 8% glycerol and 7% NCC and minimum thickness of 0.07 mm was observed with 3.17% glycerol and 5% NCC. This increase in film thickness can be attributed to the distribution of NCC as a filler and a higher content of glycerol in the resulting film [18]. These results are similar to a previous study of the effect of addition glycerol and NCC on the soy protein isolate and WPI [18,34].
Figure 2b shows the effects of varying glycerol and NCC concentrations on the tensile strength of biocomposite film. It was found that an increase in glycerol concentrations decreases the tensile strength. This can be rationalized by considering that glycerol with low molecular weight generates molecular interactions along polymer chains, increasing film flexibility while decreasing tensile properties. It would also reduce intramolecular hydrogen bonding in the network of the film. This result was similar to the chitosan–NCC film and gelatin film with the addition of glycerol [43,44]. Furthermore, glycerol acted as a plasticizer in the composite film matrix, resulting in an increased free volume and reduced network rigidity in WPI polymers. Plasticization also led to the composite films’ flexibility, reducing the tensile strength [45]. The NCC content also affected the tensile strength of the composite film, as higher NCC increased the tensile strength of the film. This result was consistent with our previous study, which used NCC as a filler in a WPI-based film [18]. The reinforcement process to increase the tensile strength by incorporating rigid nanoparticles into a polymer matrix was also ascribed to the strong interfacial interaction between NCC and WPI matrix, which resulted in the effective transfers of stress from the polymer matrix to the nanoparticles that effectively carry the load and enhance the strength of the composite films [46,47].
Figure 2c shows that higher glycerol and NCC concentrations decreased the elongation at break of the biocomposite film. The trend could be attributed to glycerol and NCC hydrophilicity, as well as the degree of thermal degradation of the NCC. The high shear stress of the polymer decreased its flexibility of films during the blending of the composite with the natural fillers, which causes the limitation of molecular chain motion in the polymer. NCC also caused non-homogeneous film matrices, which gave more dispersed granules in the films which in turn disrupted the interaction between the networks and strongly affected the elongation [48]. As the filler and plasticizer content increased, there was a probability of this phenomenon occurring during blending which would enhance the interaction between the filler and the polymer surface resulting in shorter fibers than critical grades and a reduced aspect ratio. This then directly affected the resulting composite performance and decreased tensile strength and elongation [45]. These results are also in agreement with previous studies of chitosan, sesame protein, and faba bean protein film [43,49,50].

3.4. Optimization Process of the Experiment

Glycerol and NCC concentration are the two factors in selecting optimization to make the desired composition in this study. After optimization of the experiment, there are several solutions for the physical and mechanical properties the biocomposite films, as shown in Table 7. As a result, the response was the highest obtained from the experiments. A value close to one (100%) is an acceptable value for the desirability function. The desirability function sets perimeters to find the optimal value for all the variable responses during the optimization procedure. In this study, the optimum physical and mechanical properties of the biocomposite with a desirability of 92.7% were associated with 4% glycerol and 3.5% NCC concentration. The level of this independent variable resulted in the highest thickness, tensile strength, and elongation responses, which were 0.12 mm, 6.97 MPa, and 44.65%, respectively. This study showed that the addition of high glycerol and NCC decreased the thickness, tensile strength, and elongation of the biocomposite film. Aprilia et al. also reported that the irregular structure of the reinforcing material reduced composite strength because of the bonds’ inability to support the stress transfer of the polymer matrix [51]. The weakness in the interfacial areas would decrease the effect of stress transfer from the polymer matrix to the filler component, lowering the strength of the films [39]. These results also show similarities with the study conducted by Kusmono et al., where they discovered that the strength of the composite decreased as the amount of support material increased [43].

3.5. Validation Process of the Predicted Model of Optimised Formulations

To validate the model, an experiment was carried out with three replicates for each response under the optimal conditions suggested (4% glycerol and 3.5% NCC concentration). Table 8 shows the validation of the predicted model results, which show that the thickness, tensile strength, and elongation of biocomposite films were all within the predicted range at 0.13 mm, 7.16 MPa, and 39.10%, respectively. The 95% confidence interval was found to be within the validation results for all responses. A confidence interval estimate is a set of values that the parameter is almost definitely predicted to fall inside. The confidence interval indicates that the average data for all responses will decline within this range 95% of the time. In addition, the outcomes of all responses (thickness, tensile strength, and elongation) were within the 95% prediction interval value. Due to the additional uncertainty and scattered data involved in predicting a single response as well as the mean response, the prediction interval was greater than the confidence interval. It follows that the results could be 95% certain that they included all of the responses related to these settings. Overall, the model’s validity demonstrated that preparation of WPI-based composite films under the optimum suggested glycerol and NCC compositions by RSM was achieved.

3.6. Morphological, Physical and Crystallinilty Analysis of Optimized Biocomposite Films

3.6.1. Functional Group of Optimized Biocomposite Film

The FTIR spectra of the biocomposite films were obtained in order to estimate the functional groups of the films and analyze the interactions between the film components. Figure 3 shows the biocomposite film absorptions that occurred on bands ranging from 4000 to 400 cm−1. The biocomposite films exhibited a band at approximately 3270 cm−1, which is related to the presence of the N-H bond from WPI, the stretch of the OH groups, the presence of water in all films, and the presence of OH groups on the NCC surface [12,52]. The absorption band around 3270 cm−1 shifted to a lower wavenumber as the NCC remaining in the protein sample increased. With the addition of NCC content, the peaks displayed increased in intensity. These findings indicated that the NCC addition resulted in inter- or intramolecular hydrogen bonds as well as molecular rearrangement [12]. The band at 2930 cm−1 corresponds to the C-H group’s stretching vibration and is associated with a decrease in peak intensity, incorporating primary and secondary carbon bonds (CH3 and CH2). The biocomposite films retain the main absorption of WPI films, such as C=O stretching at 1637 cm−1 (amide I), N-H bending at 1539 cm−1 (amide II), C-H deformation at 1400 cm−1, and C-N stretching (amide III) at 1232 cm−1 [10]. When compared to pure WPI film, the amide I and II peaks in biocomposite films showed a slight shift to lower wavenumber. It is implied that the polarity decreased as more hydrogen bonds formed between glycerol, NCC, and protein molecules.
Furthermore, the addition of NCC increased the intensity of the 1151–1024 cm−1 region (C-O stretching and O-H deforming vibration). Early literature found the addition of NCC to WPI film containing more O-H leads to enhanced absorbance in the region [53]. The peak at 1024 cm−1 also exhibits a small displacement because of the potential extra interactions between the plasticizer and the film structure. The peak from 1151 to 848 cm−1 attributed to absorption bands of glycerol produced peaks in the films, corresponding to the vibration of C-C and C-O bonds [54]. Comparing the spectra of pure WPI film and biocomposite films, the peak of amide I, II, and III bands were more shifted. This implies that the addition of glycerol affected the interaction between NCC and WPI in the film matrix. Generally, NCC showed good compatibility with WPI film by forming hydrogen bonds with polypeptide chains [55].

3.6.2. Morphology of Optimized Biocomposite Film

The morphology of the WPI film and biocomposite films are shown in Figure 4. As observed, pure WPI film (Figure 4ai,aii) exhibited a smooth and homogenous structure. In contrast, the films containing NCC and glycerol (Figure 4bi,bii) had rougher surfaces with the presence of pores or cavities, which could be related to the formation of channels. It is clear that the addition of NCC as a filler causes significant changes in the film structure and increases the density of crack deflection sites in biocomposite films [56]. Due to the trapped air in the film solution, some pores or bubbles were probably created during the drying process of biocomposite films. NCC as filler and glycerol as plasticizer also acted as nucleating sites for voids growing. The protein denaturation process could also cause minor aggregation on pure WPI films. This experimental evidence is consistent with the findings of the previous study [57,58].

3.6.3. Transparency of Optimized Biocomposite Film

Transparency of packaging materials portrays the products appearance and reflects the effect of NCC incorporation as a filler on the interaction matrix [53]. Table 9 shows the transparency of pure WPI film and biocomposite films. The biocomposite films were much less transparent than the pure WPI films across all wavelength ranges observed. This reduction indicates that the addition of NCC decreased the transparency of WPI films. At 800 nm, the transparency of pure WPI films was 22.5% and decreased to 13.4% with the addition of fillers. This could be due to the light path being blocked through the polymer matrix as a result of the strong interface interaction between the NCC and the WPI matrix [59]. Additionally, this decrease could be caused by the presence of the NCC particles, which increased the light scattering in the polymer matrix [10]. According to Qazanfadeh et al. [13] an NCC particle aggregation can affect the light transmission of biocomposite films by blocking the light’s passage through the protein film structure, confirming the SEM analysis results. Previous studies using a variety of biopolymer matrices, such as chitosan [43], alginate [60], casein [61], and starch [62], have observed a decrease in film transparency with the addition of cellulose nanoparticles. Furthermore, the presence of glycerol in WPI films might reduce the transparency of the biocomposite films as a result of the presence of a suitable contact area between the WPI, NCC, and glycerol structure [59].

3.6.4. Water Solubility of Optimized Biocomposite Film

The water solubilities in biocomposite films are summarized in Table 10. This shows that the pure WPI films had a higher water solubility than the biocomposite films. The addition of NCC reduced the water solubility in WPI films. The decrease in solubility might be attributed to the formation of strong structures and bonds by the mixtures added to the protein matrix [18,63]. The NCC dimension and the crystalline area have been observed as effective characteristics in the water resistance of biocomposite films [64]. Water in the WPI film barrier also decreased due to the interaction between water and the hydroxyl groups of cellulose in NCC [10]. As previously reported, the use of NCC as filler at a lower concentration can reduce the water solubility in WPI films. This can be attributed to fewer nanoparticles being dispersed in the WPI matrix and the formation of NCC agglomerates [13]. Moreover, the hydrophilic nature of protein and glycerol as materials are the reasons for the higher solubility of pure WPI films in water than the biocomposite films with the addition of NCC [65].

3.6.5. Water Vapor Permeability of Optimized Biocomposite Film

In the case of the developed biocomposite films, water vapor permeability is essential for innovative materials used for food packaging. The permeability results in Table 10 show that the addition of NCC and glycerol improved the WPI films barrier. Due to their hydrophilic nature, the water vapor barrier of protein polymer films is seen as a disadvantage of these materials. According to the previous studies, the incorporation of plasticizers and fillers in various types of micro and nanomaterials improves the biopolymers structure and characteristics [66]. When compared to pure WPI films, the addition of NCC reduced the water vapor permeability of the biocomposite films. The decrease in the water vapor permeability of the film could be attributed to NCC dispersion in the WPI polymer matrix, which favors the interference of water vapor diffusion [67]. Another possible explanation could be the hydrophilic nature of NCC as a filler in biocomposite films, reducing the water molecules adhesion [68].
The results obtained in biocomposite films appear to support those obtained in SEM analysis. This can be explained by the NCC interfering with the film morphology resulting in greater attraction and aggregation between the particles and causing the formation of less cohesive films, which may have contributed to water vapor permeation through the WPI matrix [69]. This improvement in WVP properties has previously been reported in studies using cellulose nanoparticles as a filler in whey protein-based film [10,13,37].

3.6.6. Crystallinity of Optimized Biocomposite Film

The X-ray diffraction patterns of films are related to the amorphous-crystalline structure and dependent on the crystallization rate in composite film. The XRD patterns of the pure WPI and optimal film samples are presented in Figure 5. A strong peak at around 2θ = 22° was observed in the diffractogram of the biocomposite films corresponding to the crystalline phase of (220) of the crystalline structure. The addition of glycerol and NCC resulted in similar peak locations, indicating that the morphology of the WPI crystalline structure remained unchanged [70]. Pure WPI also exhibited a broad peak at 20° and small peak at 30° to 40°, indicating the amorphous phase of the protein and also giving a relatively good crystalline degree, and can be classified as a semi-crystalline biopolymer. The semi-crystalline characteristic of WPI film was also reported by Aziz et al. and Zhang et al. [71,72]. Furthermore, the addition of NCC increased the peak intensity at 2θ = 22° as a result of the trans-crystallization effect [43]. The trans-crystallization effect is proportional to the crystal orientation of the semi-crystalline matrix to the NCC [73]. The peak around 20–23° became broader, which indicated the good compatibility between WPI and glycerol [49]. The reflection at this peak shows the major structure was amorphous and displayed molecular miscibility and interaction between the component of biocomposite film [72]. The presence of this peak also indicated that the crystalline structure of the NCC material was preserved during the biocomposite film production. The compatibility between polymers and additives can result in the formation of homogeneous films with good mechanical and physical properties, which is an important factor for biocomposite films [74].
The crystallinity indexes of WPI and biocomposite film are shown in Table 11. The result shows that the presence of NCC in the WPI matrix offered a higher crystallinity index than the WPI film without NCC. These phenomena might be attributed to the formation of new hydrogen bonds NCC and WPI, which increased the degree of film crystallinity [75]. However, the crystallinity index in this study was higher than the study reported by Hafizulhaq et al. using cellulose fibers from bengkoang as filler in starch film and Carvalho et al. using nanocellulose from Eucalyptus sp. In WPI film [69,76]. A higher crystallinity index is probably due to the crystallization of glycerol as a plasticizer in WPI film. The storage time of film before analysis can also cause crystal growth in WPI film [77].

4. Conclusions

RSM-CCD was successfully used to optimize the physical and mechanical properties of a WPI composite film by optimizing the concentrations of glycerol and NCC. The results showed that both individual variables influenced the investigated responses for physical and mechanical properties of the biocomposite film. The model suggested that the optimum condition of the biocomposite film was at a 4% glycerol and 3.5% NCC concentration. The optimal model of independent variables was numerically predicted to achieve the desired thickness, tensile strength, and elongation at break values of 0.12 mm, 6.97 MPa, and 44.65%, respectively. The corresponding validation responses were thickness (0.13 mm), tensile strength (7.16 MPa), and elongation at break (39.10%). Additionally, the results in the XRD patterns show the increase in crystallinity index and the good compatibility between WPI, glycerol, and NCC. The formation of intramolecular hydrogen bonds between WPI, NCC, and glycerol also resulted in improved integration of NCC and glycerol into the protein matrix, as supported by FTIR and SEM analysis. The addition of NCC in optimized content also slightly improved the water resistance (WS and WVP) and decreased the transparency of the biocomposite film. Hence, the development of an optimized composite film formulation produced from WPI with the addition of glycerol and NCC can be an alternative as packaging materials to replace synthetic fibers in the future. However, further research is still needed in terms of investigating the biodegradability and storage ability, as well as the toxicity and antibacterial properties of composite films, so that the materials reinforced with natural fibers can produce better properties as packaging films.

Author Contributions

Conceptualization, F.F. and S.A.; methodology, F.F. and S.A.; performed the experiments, F.F.; validation and analyzed the data, F.F., A.U. and S.A.; formal analysis, S.A.; investigation, S.A., N.A. and M.R.B.; writing—original draft preparation, F.F.; writing—review and editing, M.R.B., A.U., S.A., N.H., R.K. and N.A. All authors have read and agreed to the published version of the manuscript.

Funding

This research was funded by Universitas Syiah Kuala-based PRUUPD Research Grant No. (487/UN11/SPK/PNBP/2022). The article processing costs was supported by Universiti Malaysia Sabah.

Institutional Review Board Statement

Not applicable.

Informed Consent Statement

Not applicable.

Data Availability Statement

The data presented in this study are available on request from the corresponding author.

Acknowledgments

We acknowledged the Universitas Syiah Kuala and Universiti Malaysia Sabah for providing the grant.

Conflicts of Interest

The authors declare no conflict of interest.

References

  1. Siracusa, V.; Rocculi, P.; Romani, S.; Rosa, M.D. Biodegradable polymers for food packaging: A review. Trends Food Sci. Technol. 2008, 19, 634–643. [Google Scholar] [CrossRef]
  2. Vieira, M.G.A.; Da Silva, M.A.; Dos Santos, L.O.; Beppu, M.M. Natural-based plasticizers and biopolymer films: A review. Eur. Polym. J. 2011, 47, 254–263. [Google Scholar] [CrossRef] [Green Version]
  3. Tharanathan, R.N. Biodegradable films and composite coatings: Past, present and future. Trends Food Sci. Technol. 2003, 14, 71–78. [Google Scholar] [CrossRef]
  4. González, A.; Gastelú, G.; Barrera, G.N.; Ribotta, P.D.; Igarzabal, C. Preparation and characterization of soy protein films reinforced with cellulose nanofibers obtained from soybean by-products. Food Hydrocoll. 2019, 89, 758–764. [Google Scholar] [CrossRef]
  5. Gonzalez-Jordan, A.; Nicolai, T.; Benyahia, L. Influence of the Protein Particle Morphology and Partitioning on the Behavior of Particle-Stabilized Water-in-Water Emulsions. Langmuir 2016, 32, 7189–7197. [Google Scholar] [CrossRef]
  6. Kandasamy, S.; Yoo, J.; Yun, J.; Kang, H.-B.; Seol, K.-H.; Kim, H.-W.; Ham, J.-S. Application of Whey Protein-Based Edible Films and Coatings in Food Industries: An Updated Overview. Coatings 2021, 11, 1056. [Google Scholar] [CrossRef]
  7. Hu, Y.; Shi, L.; Ren, Z.; Hao, G.; Chen, J.; Weng, W. Characterization of emulsion films prepared from soy protein isolate at different preheating temperatures. J. Food Eng. 2021, 309, 110697. [Google Scholar] [CrossRef]
  8. Wang, L.; Auty, M.A.E.; Kerry, J.P. Physical assessment of composite biodegradable films manufactured using whey protein isolate, gelatin and sodium alginate. J. Food Eng. 2010, 96, 199–207. [Google Scholar] [CrossRef]
  9. Ahammed, S.; Liu, F.; Wu, J.; Khin, M.N.; Yokoyama, W.H.; Zhong, F. Effect of transglutaminase crosslinking on solubility property and mechanical strength of gelatin-zein composite films. Food Hydrocoll. 2021, 116, 106649. [Google Scholar] [CrossRef]
  10. Sukyai, P.; Anongjanya, P.; Bunyahwuthakul, N.; Kongsin, K.; Harnkarnsujarit, N.; Sukatta, U.; Sothornvit, R.; Chollakup, R. Effect of cellulose nanocrystals from sugarcane bagasse on whey protein isolate-based films. Food Res. Int. 2018, 107, 528–535. [Google Scholar] [CrossRef]
  11. Sothornvit, R.; Hong, S.-I.; An, D.J.; Rhim, J.-W. Effect of clay content on the physical and antimicrobial properties of whey protein isolate/organo-clay composite films. LWT Food Sci. Technol. 2010, 43, 279–284. [Google Scholar] [CrossRef]
  12. Ramos, Ó.L.; Reinas, I.; Silva, S.I.; Fernandes, J.C.; Cerqueira, M.A.; Pereira, R.N.; Vicente, A.A.; Poças, M.F.; Pintado, M.E.; Malcata, F.X. Effect of whey protein purity and glycerol content upon physical properties of edible films manufactured therefrom. Food Hydrocoll. 2013, 30, 110–122. [Google Scholar] [CrossRef] [Green Version]
  13. Qazanfarzadeh, Z.; Kadivar, M. Properties of whey protein isolate nanocomposite films reinforced with nanocellulose isolated from oat husk. Int. J. Biol. Macromol. 2016, 91, 1134–1140. [Google Scholar] [CrossRef] [PubMed]
  14. Khwaldia, K.; Perez, C.; Banon, S.; Desobry, S.; Hardy, J. Milk proteins for edible films and coatings. Crit. Rev. Food Sci. Nutr. 2004, 44, 239–251. [Google Scholar] [CrossRef] [PubMed]
  15. Asgher, M.; Qamar, S.A.; Bilal, M.; Iqbal, H. Bio-based active food packaging materials: Sustainable alternative to conventional petrochemical-based packaging materials. Food Res. Int. 2020, 137, 109625. [Google Scholar] [CrossRef] [PubMed]
  16. Garavand, F.; Rouhi, M.; Razavi, S.H.; Cacciotti, I.; Mohammadi, R. Improving the integrity of natural biopolymer films used in food packaging by crosslinking approach: A review. Int. J. Biol. Macromol. 2017, 104, 687–707. [Google Scholar] [CrossRef]
  17. Saba, N.; Tahir, P.M.; Jawaid, M. A Review on Potentiality of Nano Filler/Natural Fiber Filled Polymer Hybrid Composites. Polymers 2014, 6, 2247–2273. [Google Scholar] [CrossRef]
  18. Fitriani, F.; Aprilia, S.; Arahman, N.; Bilad, M.R.; Suhaimi, H.; Huda, N. Properties of Biocomposite Film Based on Whey Protein Isolate Filled with Nanocrystalline Cellulose from Pineapple Crown Leaf. Polymers 2021, 13, 4278. [Google Scholar] [CrossRef] [PubMed]
  19. Huq, T.; Salmieri, S.; Khan, A.; Khan, R.A.; Le Tien, C.; Riedl, B.; Fraschini, C.; Bouchard, J.; Uribe-Calderon, J.; Kamal, M.R. Nanocrystalline cellulose (NCC) reinforced alginate based biodegradable nanocomposite film. Carbohydr. Polym. 2012, 90, 1757–1763. [Google Scholar] [CrossRef]
  20. Zhao, G.; Zhou, C.; Fan, F. Preparation and Properties of Soy Protein Isolate/Cotton-Nanocrystalline Cellulose Films. Int. J. Polym. Sci. 2021, 2021, 5518136. [Google Scholar] [CrossRef]
  21. Aprilia, N.A.S.; Mulyati, S.; Alam, P.N.; Karmila; Ambarita, A.C. Characterization nano crystalline cellulose from sugarcane baggase for reinforcement in polymer composites: Effect of formic acid concentrations. IOP Conf. Ser. Mater. Sci. Eng. 2018, 345, 012033. [Google Scholar] [CrossRef] [Green Version]
  22. Fitriani, F.; Aprilia, S.; Arahman, N.; Bilad, M.R.; Amin, A.; Huda, N.; Roslan, J. Isolation and Characterization of Nanocrystalline Cellulose Isolated from Pineapple Crown Leaf Fiber Agricultural Wastes Using Acid Hydrolysis. Polymers 2021, 13, 4188. [Google Scholar] [CrossRef]
  23. Thakur, M.; Sharma, A.; Ahlawat, V.; Bhattacharya, M.; Goswami, S. Process optimization for the production of cellulose nanocrystals from rice straw derived α-cellulose. Mater. Sci. Energy Technol. 2020, 3, 328–334. [Google Scholar] [CrossRef]
  24. Aprilia, N.A.S.; Davoudpour, Y.; Zulqarnain, W.; Khalil, H.A.; Hazwan, C.M.; Hossain, M.S.; Dungani, R.; Fizree, H.M.; Zaidon, A.; Haafiz, M. Physicochemical Characterization of Microcrystalline Cellulose Extracted from Kenaf Bast. Bioresources 2016, 11, 3875–3889. [Google Scholar] [CrossRef] [Green Version]
  25. Khan, A.; Jawaid, M.; Kian, L.K.; Khan, A.A.P.; Asiri, A.M. Isolation and Production of Nanocrystalline Cellulose from Conocarpus Fiber. Polymers 2021, 13, 1835. [Google Scholar] [CrossRef]
  26. Zheng, D.; Zhang, Y.; Guo, Y.; Yue, J. Isolation and Characterization of Nanocellulose with a Novel Shape from Walnut (Juglans regia L.) Shell Agricultural Waste. Polymers 2019, 11, 1130. [Google Scholar] [CrossRef] [Green Version]
  27. Prado, K.S.; Spinacé, M.A. Isolation and characterization of cellulose nanocrystals from pineapple crown waste and their potential uses. Int. J. Biol. Macromol. 2019, 122, 410–416. [Google Scholar] [CrossRef]
  28. Fitriani; Aprilia, N.A.S.; Arahman, N. Properties of nanocrystalline cellulose from pineapple crown leaf waste. IOP Conf. Ser. Mater. Sci. Eng. 2020, 796, 12007. [Google Scholar] [CrossRef]
  29. Brinchi, L.; Cotana, F.; Fortunati, E.; Kenny, J. Production of nanocrystalline cellulose from lignocellulosic biomass: Technology and applications. Carbohydr. Polym. 2013, 94, 154–169. [Google Scholar] [CrossRef]
  30. Dick, M.; Costa, T.M.H.; Gomaa, A.; Subirade, M.; de Oliveira Rios, A.; Flôres, S.H. Edible film production from chia seed mucilage: Effect of glycerol concentration on its physicochemical and mechanical properties. Carbohydr. Polym. 2015, 130, 198–205. [Google Scholar] [CrossRef] [Green Version]
  31. Zhai, X.; Zhang, X.; Ao, H.; Yin, Y.; Li, X.; Ren, D. Preparation and characterization of whey protein isolate/chitosan/microcrystalline cellulose composite films. Packag. Technol. Sci. 2021, 34, 589–599. [Google Scholar] [CrossRef]
  32. Dixit, S.; Yadav, V.L. Optimization of polyethylene/polypropylene/alkali modified wheat straw composites for packaging application using RSM. J. Clean. Prod. 2019, 240, 118228. [Google Scholar] [CrossRef]
  33. Granato, D.; de Araújo Calado, V.M. The use and importance of design of experiments (DOE) in process modelling in food science and technology. Math. Stat. Methods Food Sci. Technol. 2014, 1, 1–18. [Google Scholar]
  34. Nandane, A.S.; Jain, R.K. Optimization of formulation and process parameters for soy protein-based edible film using response surface methodology. J. Packag. Technol. Res. 2018, 2, 203–210. [Google Scholar] [CrossRef]
  35. Kalateh-Seifari, F.; Yousefi, S.; Ahari, H.; Hosseini, S.H. Corn starch-chitosan nanocomposite film containing nettle essential oil nanoemulsions and starch nanocrystals: Optimization and characterization. Polymers 2021, 13, 2113. [Google Scholar] [CrossRef]
  36. Fan, H.Y.; Duquette, D.; Dumont, M.J.; Simpson, B.K. Salmon skin gelatin-corn zein composite films produced via crosslinking with glutaraldehyde: Optimization using response surface methodology and characterization. Int. J. Biol. Macromol. 2018, 120, 263–273. [Google Scholar] [CrossRef]
  37. Alizadeh-Sani, M.; Khezerlou, A.; Ehsani, A. Fabrication and characterization of the bionanocomposite film based on whey protein biopolymer loaded with TiO2 nanoparticles, cellulose nanofibers and rosemary essential oil. Ind. Crops Prod. 2018, 124, 300–315. [Google Scholar] [CrossRef]
  38. Segal, L.; Creely, J.J.; Martin, A.E.; Conrad, C.M. An Empirical Method for Estimating the Degree of Crystallinity of Native Cellulose Using the X-Ray Diffractometer. Text. Res. J. 1959, 29, 786–794. [Google Scholar] [CrossRef]
  39. Penjumras, P.; Abdul Rahman, R.; Talib, R.A.; Abdan, K. Response Surface Methodology for the Optimization of Preparation of Biocomposites Based on Poly(lactic acid) and Durian Peel Cellulose. Sci. World J. 2015, 2015, 293609. [Google Scholar] [CrossRef] [Green Version]
  40. Lv, C.; Wang, Y.; Wang, L.-j.; Li, D.; Adhikari, B. Optimization of production yield and functional properties of pectin extracted from sugar beet pulp. Carbohydr. Polym. 2013, 95, 233–240. [Google Scholar] [CrossRef]
  41. Said, N.S.; Sarbon, N.M. Response surface methodology (RSM) of chicken skin gelatin based composite films with rice starch and curcumin incorporation. Polym. Test. 2020, 81, 106161. [Google Scholar] [CrossRef]
  42. Chang, B.P.; Akil, H.M.; Affendy, M.G.; Khan, A.; Nasir, R.B.M. Comparative study of wear performance of particulate and fiber-reinforced nano-ZnO/ultra-high molecular weight polyethylene hybrid composites using response surface methodology. Mater. Des. 2014, 63, 805–819. [Google Scholar] [CrossRef]
  43. Wildan, M.W.; Lubis, F. Fabrication and Characterization of Chitosan/Cellulose Nanocrystal/Glycerol Bio-Composite Films. Polymers 2021, 13, 1096. [Google Scholar]
  44. Nazmi, N.N.M.; Sarbon, N.M. Response Surface Methodology on development and formulation optimisation of chicken skin gelatine film blended with carboxymethyl cellulose as affected by varying plasticiser concentrations. Int. Food Res. J. 2019, 26, 47–57. [Google Scholar]
  45. Wongphan, P.; Khowthong, M.; Supatrawiporn, T.; Harnkarnsujarit, N.J.F.P.; Life, S. Novel edible starch films incorporating papain for meat tenderization. Shelf Life 2022, 31, 100787. [Google Scholar] [CrossRef]
  46. Mukurumbira, A.R.; Mellem, J.J.; Amonsou, E. Effects of amadumbe starch nanocrystals on the physicochemical properties of starch biocomposite films. Carbohydr. Polym. 2017, 165, 142–148. [Google Scholar] [CrossRef]
  47. Phothisarattana, D.; Harnkarnsujarit, N. Characterizations of Cassava Starch and Poly (butylene adipate-co-terephthalate) Blown Film with Silicon Dioxide Nanocomposites. Int. J. Food Sci. Technol. 2022, 57, 5078–5089. [Google Scholar] [CrossRef]
  48. Phothapaeree, N.; Jarusaksakul, N.; Somwangthanaroj, A.; Tananuwong, K. Influence of packaging and storage conditions on quality parameters and shelf life of solar-dried banana. Songklanakarin J. Sci. Technol. 2017, 39, 253–260. [Google Scholar] [CrossRef]
  49. Sharma, L.; Singh, C. Sesame protein based edible films: Development and characterization. Food Hydrocoll. 2016, 61, 139–147. [Google Scholar] [CrossRef]
  50. Saremnezhad, S.; Azizi, M.H.; Barzegar, M.; Abbasi, S.; Ahmadi, E. Properties of a new edible film made of faba bean protein isolate. J. Agric. Sci. Technol. 2011, 13, 181–192. [Google Scholar]
  51. Aprilia, S.; Syamsuddin, Y.; Razali, N.; Fitriani, F.; Amin, A.; Guswara, F.; Ihsan, F. Studies on degradation of rice husk ash filled in polypropylene composite films under natural weathering condition. J. Phys. Conf. Ser. 2019, 1402, 055009. [Google Scholar] [CrossRef]
  52. Lara, B.R.B.; de Andrade, P.S.; Guimarães Junior, M.; Dias, M.V.; Alcântara, L.A.P. Novel Whey Protein Isolate/Polyvinyl Biocomposite for Packaging: Improvement of Mechanical and Water Barrier Properties by Incorporation of Nano-silica. J. Polym. Environ. 2021, 29, 2397–2408. [Google Scholar] [CrossRef]
  53. Jiang, S.j.; Zhang, T.; Song, Y.; Qian, F.; Tuo, Y.; Mu, G. Mechanical properties of whey protein concentrate based film improved by the coexistence of nanocrystalline cellulose and transglutaminase. Int. J. Biol. Macromol. 2019, 126, 1266–1272. [Google Scholar] [CrossRef] [PubMed]
  54. Guerrero, P.; Retegi, A.; Gabilondo, N.; De la Caba, K. Mechanical and thermal properties of soy protein films processed by casting and compression. J. Food Eng. 2010, 100, 145–151. [Google Scholar] [CrossRef]
  55. Yu, Z.; Sun, L.; Wang, W.; Zeng, W.; Mustapha, A.; Lin, M. Soy protein-based films incorporated with cellulose nanocrystals and pine needle extract for active packaging. Ind. Crops Prod. 2018, 112, 412–419. [Google Scholar] [CrossRef]
  56. Li, C.; Luo, J.; Qin, Z.; Chen, H.; Gao, Q.; Li, J. Mechanical and thermal properties of microcrystalline cellulose-reinforced soy protein isolate–gelatin eco-friendly films. RSC Adv. 2015, 5, 56518–56525. [Google Scholar] [CrossRef]
  57. Oymaci, P.; Altinkaya, S.A. Improvement of barrier and mechanical properties of whey protein isolate based food packaging films by incorporation of zein nanoparticles as a novel bionanocomposite. Food Hydrocoll. 2016, 54, 1–9. [Google Scholar] [CrossRef] [Green Version]
  58. Al-Hassan, A.; Norziah, M. Starch–gelatin edible films: Water vapor permeability and mechanical properties as affected by plasticizers. Food Hydrocoll. 2012, 26, 108–117. [Google Scholar] [CrossRef]
  59. Hejazi, M.; Behzad, T.; Heidarian, P.; Nasri-Nasrabadi, B. A study of the effects of acid, plasticizer, cross-linker, and extracted chitin nanofibers on the properties of chitosan biofilm. Compos. Part A Appl. Sci. Manuf. 2018, 109, 221–231. [Google Scholar] [CrossRef]
  60. Abdollahi, M.; Alboofetileh, M.; Rezaei, M.; Behrooz, R. Comparing physico-mechanical and thermal properties of alginate nanocomposite films reinforced with organic and/or inorganic nanofillers. Food Hydrocoll. 2013, 32, 416–424. [Google Scholar] [CrossRef]
  61. Pereda, M.; Amica, G.; Rácz, I.; Marcovich, N.E. Structure and properties of nanocomposite films based on sodium caseinate and nanocellulose fibers. J. Food Eng. 2011, 103, 76–83. [Google Scholar] [CrossRef]
  62. Tibolla, H.; Czaikoski, A.; Pelissari, F.; Menegalli, F.; Cunha, R. Starch-based nanocomposites with cellulose nanofibers obtained from chemical and mechanical treatments. Int. J. Biol. Macromol. 2020, 161, 132–146. [Google Scholar] [CrossRef]
  63. Zolfi, M.; Khodaiyan, F.; Mousavi, M.; Hashemi, M. Development and characterization of the kefiran-whey protein isolate-TiO2 nanocomposite films. Int. J. Biol. Macromol. 2014, 65, 340–345. [Google Scholar] [CrossRef] [PubMed]
  64. Chen, Y.; Liu, C.; Chang, P.R.; Anderson, D.P.; Huneault, M.A. Pea starch-based composite films with pea hull fibers and pea hull fiber-derived nanowhiskers. Polym. Eng. Sci. 2009, 49, 369–378. [Google Scholar] [CrossRef]
  65. El-Wakil, N.A.; Hassan, E.A.; Abou-Zeid, R.E.; Dufresne, A. Development of wheat gluten/nanocellulose/titanium dioxide nanocomposites for active food packaging. Carbohydr. Polym. 2015, 124, 337–346. [Google Scholar] [CrossRef] [PubMed]
  66. Calva-Estrada, S.J.; Jiménez-Fernández, M.; Lugo-Cervantes, E. Protein-Based Films: Advances in the Development of Biomaterials Applicable to Food Packaging. Food Eng. Rev. 2019, 11, 78–92. [Google Scholar] [CrossRef]
  67. Dias, M.V.; Azevedo, V.M.; Santos, T.A.; Pola, C.C.; Lara, B.R.B.; Borges, S.V.; Soares, N.F.F.; Medeiros, É.A.A.; Sarantópoulous, C. Effect of active films incorporated with montmorillonite clay and α-tocopherol: Potential of nanoparticle migration and reduction of lipid oxidation in salmon. Packag. Technol. Sci. 2019, 32, 39–47. [Google Scholar] [CrossRef] [Green Version]
  68. Duval, A.; Molina-Boisseau, S.; Chirat, C. Comparison of Kraft lignin and lignosulfonates addition to wheat gluten-based materials: Mechanical and thermal properties. Ind. Crop. Prod. 2013, 49, 66–74. [Google Scholar] [CrossRef]
  69. Carvalho, R.A.; de Oliveira, A.C.S.; Santos, T.A.; Dias, M.V.; Yoshida, M.I.; Borges, S.V. WPI and cellulose nanofibres bio-nanocomposites: Effect of thyme essential oil on the morphological, mechanical, barrier and optical properties. J. Polym. Environ. 2020, 28, 231–241. [Google Scholar] [CrossRef]
  70. Bumbudsanpharoke, N.; Wongphan, P.; Promhuad, K.; Leelaphiwat, P.; Harnkarnsujarit, N. Morphology and permeability of bio-based poly(butylene adipate-co-terephthalate) (PBAT), poly(butylene succinate) (PBS) and linear low-density polyethylene (LLDPE) blend films control shelf-life of packaged bread. Food Control 2022, 132, 108541. [Google Scholar] [CrossRef]
  71. Aziz, S.G.-G.; Almasi, H.J.F.; Technology, B. Physical characteristics, release properties, and antioxidant and antimicrobial activities of whey protein isolate films incorporated with thyme (Thymus vulgaris L.) extract-loaded nanoliposomes. Food Bioprocess Technol. 2018, 11, 1552–1565. [Google Scholar] [CrossRef]
  72. Zhang, X.; Zhao, Y.; Li, Y.; Zhu, L.; Fang, Z.; Shi, Q. Physicochemical, mechanical and structural properties of composite edible films based on whey protein isolate/psyllium seed gum. Int. J. Biol. Macromol. 2020, 153, 892–901. [Google Scholar] [CrossRef] [PubMed]
  73. Gray, D.G. Transcrystallization of polypropylene at cellulose nanocrystal surfaces. Cellulose 2008, 15, 297–301. [Google Scholar] [CrossRef]
  74. Mohammadian, M.; Moghaddam, A.D.; Sharifan, A.; Dabaghi, P.; Hadi, S. Characterization, Structural, physico-mechanical, and bio-functional properties of whey protein isolate-based edible films as affected by enriching with nettle (Urtica dioica L.) leaf extract. J. Food Meas. Charact. 2021, 15, 4051–4060. [Google Scholar] [CrossRef]
  75. Ghanbarzadeh, B.; Oleyaei, S.A.; Almasi, H. Nanostructured materials utilized in biopolymer-based plastics for food packaging applications. Crit. Rev. Food Sci. Nutr. 2015, 55, 1699–1723. [Google Scholar] [CrossRef] [PubMed]
  76. Hafizulhaq, F.; Abral, H.; Kasim, A.; Arief, S.; Affi, J. Moisture absorption and opacity of starch-based biocomposites reinforced with cellulose fiber from bengkoang. Fibers 2018, 6, 62. [Google Scholar] [CrossRef] [Green Version]
  77. Jooyandeh, H. Whey protein films and coatings: A review. Pak. J. Nutr. 2011, 10, 296–301. [Google Scholar] [CrossRef] [Green Version]
Figure 1. Schematic illustration of nanocrystalline cellulose isolation and biocomposite film preparation.
Figure 1. Schematic illustration of nanocrystalline cellulose isolation and biocomposite film preparation.
Polymers 14 03006 g001
Figure 2. Response surface plot of (a) thickness; (b) tensile strength; and elongation (c) as influenced by the addition of glycerol and NCC.
Figure 2. Response surface plot of (a) thickness; (b) tensile strength; and elongation (c) as influenced by the addition of glycerol and NCC.
Polymers 14 03006 g002
Figure 3. FTIR spectra of pure whey protein film and biocomposite film.
Figure 3. FTIR spectra of pure whey protein film and biocomposite film.
Polymers 14 03006 g003
Figure 4. SEM image on the surface (a) and cross section (b) of pure WPI film (i) and biocomposite film (ii).
Figure 4. SEM image on the surface (a) and cross section (b) of pure WPI film (i) and biocomposite film (ii).
Polymers 14 03006 g004
Figure 5. X-ray diffraction patterns of biocomposite film.
Figure 5. X-ray diffraction patterns of biocomposite film.
Polymers 14 03006 g005
Table 1. Coded levels of variable glycerol and NCC.
Table 1. Coded levels of variable glycerol and NCC.
VariableCoded Levels
−α−10 a+1
X1: glycerol concentrations (%)3.174688.82
X2: NCC concentrations (%)2.173577.82
a Center point; k = 2 (two independent variables); α = 1.414.
Table 2. The configuration of the response surface methodology–center composite design for biocomposite films.
Table 2. The configuration of the response surface methodology–center composite design for biocomposite films.
TrialCoded VariablesActual Variables
X1X2X1 (%)X2 (%)
10065
2−1147
3−1−143
408.825
5−α03.175
60065
71187
81−183
90−α62.17
100065
11067.82
120065
130065
Table 3. The responses of the central composite design parameters of the biocomposite films.
Table 3. The responses of the central composite design parameters of the biocomposite films.
TrialIndependent VariablesResponses
Glycerol
Concentrations
(%)
NCCC
oncentrations
(%)
Thickness *
(mm)
Tensile Strength * (MPa)Elongation * (%)
1650.23 ± 0.053.92 ± 0.9835.88 ± 14.29
2470.12 ± 0.013.60 ± 0.5718.29 ± 3.84
3430.09 ± 0.026.87 ± 0.2240.29 ± 3.11
48.8250.15 ± 0.031.64 ± 0.574.71 ± 1.70
53.1750.09 ± 0.017.85 ± 0.1141.13 ± 4.92
6650.19 ± 0.034.03 ± 0.6236.54 ± 11.83
7870.24 ± 0.072.62 ± 0.576.71 ± 3.72
8830.07 ± 0.011.96 ± 0.3818.67 ± 7.32
962.170.12 ± 0.022.62 ± 0.5742.92 ± 3.35
10650.21 ± 0.034.12 ± 0.3430.92 ± 9.54
1167.820.16 ± 0.031.96 ± 0.2314.80 ± 5.25
12650.19 ± 0.034.92 ± 0.1236.81 ± 13.93
13650.21 ± 0.034.92 ± 0.1236.87 ± 13.57
* Values are expressed as mean ± standard deviation.
Table 4. Variance analysis for the quadratic thickness model in biocomposite films.
Table 4. Variance analysis for the quadratic thickness model in biocomposite films.
SourceSum of SquaresDFMean SquaresF ValueProb > F
Model0.037450.007513.400.0018 (significant)
Residual0.003970.0006
Lack-of-fit0.002930.00103.860.1126 (not significant)
Pure error0.001040.0003
Total0.041312
Standard deviation = 0.0236; mean = 0.1583; R2 = 0.9054; and adequate precision = 8.6184.
Table 5. Variance analysis for the quadratic tensile strength model in biocomposite films.
Table 5. Variance analysis for the quadratic tensile strength model in biocomposite films.
SourceSum of SquaresDFMean SquaresF ValueProb > F
Model40.0558.0122.260.0004 significant
Residual2.5270.3598
Lack-of-fit1.5330.50992.060.2480 not significant
Pure error0.989140.2473
Total42.5712
Standard deviation = 0.5999; mean = 3.93; R2 = 0.9408; and adequate precision = 15.1960.
Table 6. Variance analysis for the quadratic elongation at break model in biocomposite films.
Table 6. Variance analysis for the quadratic elongation at break model in biocomposite films.
SourceSum of SquaresDFMean SquaresF ValueProb > F
Model2077.395415.4824.280.0003 significant
Residual119.80717.11
Lack-of-fit94.04331.354.870.0802 not significant
Pure error25.7746.44
Total2197.1912
Standard deviation = 4.14; mean = 28.04; R2 = 0.9455; and adequate precision = 14.3242.
Table 7. The coefficients of regression and the probability values of approximate model for variables responses.
Table 7. The coefficients of regression and the probability values of approximate model for variables responses.
TermThicknessTensile StrengthElongation at Break
CoefficientProbabilityCoefficientProbabilityCoefficientProbability
Constant0.20640.00184.380.000435.410.0003
X1: Glycerol0.02350.0262−1.83<0.0001−10.590.0002
X2: NCC0.03280.0057−0.44230.0755−9.210.0004
X1X20.03640.01780.98120.01362.510.2643
X12−0.04300.00200.23990.3265−7.470.0021
X22−0.03520.0056−0.98580.0034−4.500.0241
Table 8. The acceptable range and validation for optimized biocomposite films.
Table 8. The acceptable range and validation for optimized biocomposite films.
Response95% CI95% PIValidation
LowHighLowHighExperimental Value
Thickness (mm)0.060.150.040.180.13 ± 0.01
Tensile strength (MPa)5.778.015.088.707.16 ± 0.33
Elongation (%)38.0153.4833.2858.2239.10 ± 2.90
CI = confidence interval; PI = prediction interval.
Table 9. Transparency of of WPI and biocomposite films.
Table 9. Transparency of of WPI and biocomposite films.
FilmWavelength (nm)
300400500600700800
WPI06.53 ± 0.1010.83 ± 0.0615.53 ± 0.0918.05 ± 0.5522.51 ± 0.25
WPI/NCC/Glycerol03.35 ± 0.094.99 ± 0.117.59 ± 0.0311.24 ± 0.2713.46 ± 0.46
Table 10. Water solubility and water vapor permeability of WPI and biocomposite films.
Table 10. Water solubility and water vapor permeability of WPI and biocomposite films.
FilmWS (%) *WVP (×10−11 g/m.s.Pa) *
WPI30.21 ± 0.102.21 ± 0.10
WPI/NCC/Glycerol27.15 ± 0.162.17 ± 0.08
* Value are expressed as mean ± standard deviation.
Table 11. Crystallinity index of WPI and biocomposite films.
Table 11. Crystallinity index of WPI and biocomposite films.
FilmCrystallinity Index (%)
WPI74.82
WPI/Glycerol76.49
WPI/NCC/Glycerol81.14
Publisher’s Note: MDPI stays neutral with regard to jurisdictional claims in published maps and institutional affiliations.

Share and Cite

MDPI and ACS Style

Fitriani, F.; Aprilia, S.; Bilad, M.R.; Arahman, N.; Usman, A.; Huda, N.; Kobun, R. Optimization of Biocomposite Film Based on Whey Protein Isolate and Nanocrystalline Cellulose from Pineapple Crown Leaf Using Response Surface Methodology. Polymers 2022, 14, 3006. https://doi.org/10.3390/polym14153006

AMA Style

Fitriani F, Aprilia S, Bilad MR, Arahman N, Usman A, Huda N, Kobun R. Optimization of Biocomposite Film Based on Whey Protein Isolate and Nanocrystalline Cellulose from Pineapple Crown Leaf Using Response Surface Methodology. Polymers. 2022; 14(15):3006. https://doi.org/10.3390/polym14153006

Chicago/Turabian Style

Fitriani, Fitriani, Sri Aprilia, Muhammad Roil Bilad, Nasrul Arahman, Anwar Usman, Nurul Huda, and Rovina Kobun. 2022. "Optimization of Biocomposite Film Based on Whey Protein Isolate and Nanocrystalline Cellulose from Pineapple Crown Leaf Using Response Surface Methodology" Polymers 14, no. 15: 3006. https://doi.org/10.3390/polym14153006

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.

Article Metrics

Back to TopTop