Next Article in Journal
Co-Sintering of Li1.3Al0.3Ti1.7(PO4)3 and LiFePO4 in Tape-Casted Composite Cathodes for Oxide Solid-State Batteries
Next Article in Special Issue
An Extended Kalman Filter Design for State-of-Charge Estimation Based on Variational Approach
Previous Article in Journal
Mechanical and Optical Characterization of Lithium-Ion Battery Cell Components/Cross-Ply Lamination Effect
Previous Article in Special Issue
Online State-of-Health Estimation for Fast-Charging Lithium-Ion Batteries Based on a Transformer–Long Short-Term Memory Neural Network
 
 
Font Type:
Arial Georgia Verdana
Font Size:
Aa Aa Aa
Line Spacing:
Column Width:
Background:
Article

Assessment of Health Indicators to Detect the Aging State of Commercial Second-Life Lithium-Ion Battery Cells through Basic Electrochemical Cycling

by
Emanuele Michelini
*,
Patrick Höschele
,
Syed Muhammad Abbas
,
Christian Ellersdorfer
and
Jörg Moser
Vehicle Safety Institute, Graz University of Technology, 8010 Graz, Austria
*
Author to whom correspondence should be addressed.
Batteries 2023, 9(11), 542; https://doi.org/10.3390/batteries9110542
Submission received: 25 September 2023 / Revised: 31 October 2023 / Accepted: 31 October 2023 / Published: 1 November 2023
(This article belongs to the Special Issue Advances in Battery Status Estimation and Prediction)

Abstract

:
Upon reaching certain limits, electric vehicle batteries are replaced and may find a second life in various applications. However, the state of such batteries in terms of aging and safety remains uncertain when they enter the second-life market. The aging mechanisms within these batteries involve a combination of processes, impacting their safety and performance. Presently, direct health indicators (HIs) like state of health (SOH) and internal resistance increase are utilized to assess battery aging, but they do not always provide accurate indications of the battery’s health state. This study focuses on analyzing various HIs obtained through a basic charging–discharging cycle and assessing their sensitivity to aging. Commercial 50 Ah pouch cells with different aging histories were tested, and the HIs were evaluated. Thirteen HIs out of 31 proved to be highly aging-sensitive, and thus good indicators. Namely, SOH upon charging and discharging, Coulombic efficiency, constant current discharge time, voltage relaxation profile trend, voltage–charge area upon discharging, hysteresis open circuit voltage HIs, and temperature difference between the tabs upon charging. The findings offer valuable insights for developing robust qualification algorithms and reliable battery health monitoring systems for second-life batteries, ensuring safe and efficient battery operation in diverse second-life applications.

1. Introduction

Lithium-ion batteries are widely used in electric vehicles (EVs), due to their lifetime, performance, and high energy density [1]. The EV’s battery is replaced from the vehicle once certain limits are reached, e.g., 80% capacity retention [2,3]. The removed battery can be repurposed for a second-life application [4]. However, accurately determining the aging and safety state of these batteries upon arrival at refurbishing companies remains a challenge. The aging of lithium-ion batteries is a complex phenomenon influenced by a combination of physical and chemical mechanisms typically summarized by the scientific literature in three categories, i.e., loss of active material (LAM), loss of lithium inventory (LLI), and internal resistance increase (IRI) [5,6,7,8,9]. The aging occurring within the cell may pose serious safety risks, e.g., thermal runaway is triggered at lower temperatures [10,11,12] and the increased plated lithium may more likely lead to an internal short-circuit [13,14]. In addition, the legal framework of second-life batteries is still undefined [15]. Consequently, the development of a standardized procedure to identify the state, especially in terms of safety, of these second-life batteries becomes imperative.
Typically, direct health indicators (HIs), i.e., state of health (SOH) and IRI, are used to assess the battery’s aging status [16]. However, these indicators merely provide information on the available capacity of the battery, but not an accurate indication of the battery’s aging or safety state [7]. In fact, a degradation mechanism is not always correlated with the capacity fade of the cell. For example, there may be LAM in the absence of LLI and without capacity fade being observed in the cell [17,18,19]. Nonetheless, other HIs are sensitive to aging and can give additional information on the battery state.
To address the aforementioned limitations and gain deeper insights into battery aging, this paper introduces a novel comprehensive assessment of HIs derived through a basic charging–discharging cycle, evaluating their sensitivity to aging. The selection of HIs is based on existing literature and focuses on HIs based on quantities typically measured in battery packs, namely, current, voltage, and temperature. Aging affects the electro-thermal behavior of the cell, for example, noticeable changes occur in the voltage–time curve. Aged NMC cells charged in a constant current (CC) reach the constant-voltage (CV) phase more rapidly [20,21] and increase the duration of the CV phase [22]. Furthermore, with aging, the extracted charge compared to the inserted charge is reduced [23]. This shorter CV phase also affects the current–time curve, resulting in a steeper current decrease in fresh cells [24]. Aging also influences the voltage relaxation profile (VRP), which is extracted during the relaxation time after charging. Aged cells require more time to reach a relaxed voltage, which is lower compared to fresh cells [25,26]. Similarly, the voltage–charge behavior is affected by aging, with aged cells showing a reduced area below the voltage–charge curve [18]. The open circuit voltage (OCV) curve is also impacted by aging, leading to steeper curves and higher voltages [27]. Finally, aged cells generate more heat [28] and display greater thermal heterogeneities across the cell [29]. Thus, considering the input from the literature, the analysis is based on seven curves extracted during the basic charging–discharging cycle. These curves yield a catalog of 31 distinct HIs listed in Table 1. The HIs and how they are computed are described in more detail in Section 2.
The findings gained from these sensitive HIs hold valuable implications for the development of qualification algorithms, particularly for second-life batteries. Furthermore, the simplicity of the evaluation procedure facilitates its replicability with other cells, enhancing its practicality and potential for widespread application in the field of battery-aging research.

2. Materials and Methods

The tested battery cells were commercial 50 Ah pouch cells with nickel–manganese–cobalt oxide cathode (NMC111), graphite anode, and SEPARION® separator [31], intended for use in an EV module. The cell has a nominal voltage of 3.65 V and a specific energy of 147 Wh/kg. For the analysis, cells with different aging histories were tested: F1, F2, A1, and A2, see Table 2. Cells F1 and F2 were nearly not electrically cycled while A1 and A2 were electrically cycled inside commercial vehicles. This selection enabled us to have two distinct non-electrically aged cells (F1 and F2) as references to be compared with the two differently electrically aged cells (A1 and A2) to see how the different aging affects the investigated HIs.
One cell from each aging history was tested (F1, F2, A1, A2), except for F2, where three cells extracted from different positions in the module were tested (F2_C1, F2_C2, F2_C3), and the test on one of the cells of F2 was repeated 3 times to check the repeatability of the measurement.
The cells were charged with CC-CV (constant-current–constant-voltage) from 0% state of charge (SOC) to 100% SOC with constant-current (CC) of 25 A (C/2) until the upper cut-off voltage of 4.2 V. Once the cut-off voltage is reached, the cells were charged in CV with a cut-off current of 2.5 A (C/20). Then, after 2 h of waiting time during which the VRP was obtained, the cells were discharged with a CC of 25 A (C/2) until the lower cut-off voltage of 3.0 V. During cycling, the temperature was measured using thermocouples near the tabs. The cells were charged and discharged using a bi-directional power supply (EA-PSB 9060-120 3U), which was also employed for measuring the current. The voltage was measured using a sense cable via the NI9229 Module, while the temperature values were obtained using K-type thermocouples via the NI9213 Module. Both NI modules were controlled through the NI Compact-DAQ-9178.

2.1. Voltage–Time Behavior upon Cycling

In the voltage–time curves, the following HIs are measured: SOH upon charging and discharging, Coulombic Efficiency (CE), Constant Current Charge Time (CCCT), Constant Voltage Charge Time (CVCT), CVCT/CCCT, and Constant Current Discharge time (CCDT). The measured HIs are shown in Figure 1.
There are several techniques for estimating SOH, yet due to its simplicity, one of the most widely used methods is coulomb counting [32]. The coulomb counting method is based on the integration of the current I over time t during a full charge or discharge to estimate the inserted or extracted capacity from the battery. The SOH is the ratio of the inserted or extracted charge (depending if it is measured upon charging or discharging) over the rated capacity of the cell C R A T E D , see Equation (1).
S O H = 1 C R A T E D I d t
CE compares the charge inserted during battery charging C C H A R with the charge extracted during discharging C D I S in order to depict the completeness of the process [23], as shown in Equation (2).
C E = C C H A R C D I S
The CCCT refers to the time needed to reach the CV phase upon charging. Similarly, CCDT consists in the time taken during discharge to reach the lower cut-off voltage. The CVCT is the time spent during charging in the CV phase, see Figure 1.

2.2. Current-Time Behavior during the CV Charging Phase

From the CV phase upon charging, it is possible also to extract the Constant Voltage Current Profile (CVCP), shown in Figure 2.
During the CV phase, the current decreases following an exponential trend with time. The coefficients a1 and a2 of the regression function shown in Equation (3) can be calculated and compared. The precision of the regression is assessed through the coefficient of determination R2, calculated using the Residual Sum of Squares (RSS) and the Total Sum of Squares (TSS).
I C V t = a 1 · e a 2 · t , R 2 = 1 R S S T S S

2.3. Voltage-Time Behavior at the End of Charging While Waiting-Voltage Relaxation Profile (VRP)

The VRP is the voltage trend during the waiting time at the end of charging, shown in Figure 3.
The VRP yields two extracted HIs: the relaxed voltage, measured after a two-hour waiting period at the end of charging, and the VRP slope, representing the voltage trend between the first and second hour, calculated with Equation (4).
V o l t a g e   s l o p e = V 60 V 120 3600

2.4. Voltage–Charge Behavior upon Cycling

The voltage–charge curves are shown in Figure 4, with the extracted HIs.
The considered HIs refer to the area under the voltage–charge curve A V Q . The area is computed using Equation (5). with V as voltage and Q as capacity.
A V Q = V d Q

2.5. Hysteresis Voltage Profile–Open Circuit Voltage (OCV) Approximation

Two techniques are commonly used for measuring the OCV curve. The first is “step-wise OCV”, which consists of charging up to a certain SOC and then measuring the voltage after a suitable relaxation time [30,33]. The second is “low-current OCV”, which consists of charging the battery with a very low current (i.e., <0.1 C) and considering the battery voltage in a state of quasi-equilibrium. Both of these techniques, however, are time-consuming. An alternative that requires less time is “hysteresis OCV”, which consists of averaging the charge and discharge voltage profile over the capacity [34,35,36] while using higher C-rates and no waiting time. The voltage hysteresis is affected by C-rate, particle size, and electrode thickness [37].
For the OCV approximation, the voltage versus capacity curve during charging is averaged with the curve obtained during discharging (black lines), as shown in Figure 5.
From the hysteresis OCV curve, five HIs are extracted. Namely the voltage at 15 Ah (30% SOC), 25 Ah (50% SOC), 25 Ah (70% SOC), the slope (i.e., the change in charge per voltage) between 15 and 25 Ah, and between 25 and 35 Ah. The slope is computed using Equation (6).
S l o p e x y = Q x y V x y

2.6. Thermal Evolution upon Cycling

The thermal behavior of the cell is also investigated. As shown in Figure 6 the HIs considered are the maximum absolute temperature reached and the temperature rise, i.e., the maximum minus the minimum temperature measured on either the positive or the negative tab of the cell.
Additionally, the maximum and the average temperature differences over time between the temperature measured on the positive tab and the negative tab are considered.

2.7. Repeatability, Sensitivity, and Monotonicity Assessment

In order to be considered valid HIs, the parameters under investigation must meet certain requirements, namely, independence of starting point, and the possibility of absolute number extraction. It is important to guarantee the independence of starting point since the method is designed for second-life batteries, additionally, the scenario in which no information is available on the state of the battery at the beginning (and during) its first life must be considered. The only information available is the basic information contained in each battery datasheet such as the nominal capacity and the upper and lower voltage limit.
On the other hand, the ability to extract absolute numbers offers a simplified approach to comparing cells by utilizing a single absolute number as a reference. This, in turn, simplifies the implementation of the parameter within algorithms or models.
Furthermore, an evaluation of the HIs is carried out considering repeatability, sensitivity, and monotonicity.
Repeatability refers to the consistency of the HI measurements. A HI with good repeatability will produce consistent results when measured multiple times under the same conditions. Hence, the same HI measured under the same conditions must not spread. Repeatability is defined by Equation (7).
R e p e a t a b i l i y = σ c y c l e s F 2 _ C 3 σ m o d u l e F 2
With σ referring to standard deviation, the numerator refers to the repetitions conducted on the cell F2_C3 (see Table 2), and the denominator to all the measurements conducted on the cells extracted from F2 (see Table 2). The standard deviation is calculated using Equation (8).
σ = x i x ¯ 2 N
In the formula, x i refers to each data point, x ¯ is the dataset average and N is the population size, i.e., the number of measurements included in the dataset.
A lower Repeatability value corresponds to a smaller spread of the values obtained by measuring the same cell under the same conditions than the values measured within the module itself, and thus to a higher score. The application is evaluated for Repeatability according to the evaluation scheme shown in Table 3.
Sensitivity is a measure of how well a HI can reflect changes in battery aging. The difference between the HI measured for the aged cells and for the non-electrically aged cells must be greater than the spread of the measurements found for the cells extracted from the module containing non-electrically aged cells F2. Sensitivity is defined by Equation (9).
S e n s i t i v i t y = σ m o d u l e F 2 σ d a t a s e t
The denominator refers to the standard deviation of the whole dataset. A lower Sensitivity value corresponds to a lower spread of the values obtained by measuring the cells in the same non-electrically aged module compared to the values measured in the whole dataset, indicative of a change of the HI with aging, and thus to a better score. The application is evaluated for repeatability according to the evaluation scheme shown in Table 3.
Monotonicity refers to a HI’s consistent increase or decrease with changes in battery aging. In other words, as batteries age, the measured HI should consistently move in the same direction, either increasing or decreasing, compared to non-electrically aged cells. Monotonicity is defined by Equation (10).
M o n o t o n i c i t y = ( F 1 A 1 ) ( F 1 A 2 )
F1, A1, and A2 refer to the absolute value of the HI measured on the cell extracted from the corresponding cell ID (see Table 2). If the value of Monotonicity is less than zero, it implies that the criterion is not met and the HI is not considered appropriate as HI and the score will be zero as shown in Table 4.
An example showing the approach for the extrapolation of Repeatability, Sensitivity, and Monotonicity is provided in Appendix A.
Multiplying the values of Repeatability, Sensitivity, and Monotonicity gives the overall score of the HI under analysis, as shown in Equation (11).
F i n a l   s c o r e = S c o r e R e p e a t a b i l i t y · S c o r e S e n s i t i v i t y · S c o r e M o n o t o n i c i t y
This allows the ranking of the HIs under investigation. All HIs with values that are at or above the upper quartile value will be considered good aging-sensitivity HIs, and the remaining poor aging-sensitivity HIs.

3. Results and Discussion

3.1. Voltage–Time Behavior upon Cycling

The SOH is measured during both the charging and discharging of the cell using Equation (1). The voltage over time charging and discharging curves are shown in Figure 7.
The SOH values measured upon charging and discharging follow a similar pattern, the absolute measured values are shown in Table 5. The table in the “Average” column presents the arithmetic mean of all cells with the same aging history. For F1, A1, and A2, where only one measurement was taken, the average corresponds to that specific measurement. In the case of F2, the average is calculated from the six measurements in the table. The same approach was consistently applied in subsequent tables.
The SOH is an indicator of the cell’s capacity retention. The capacity of a cell fades with aging mainly due to LAM and LLI [38,39]. F1 and F2 exhibit the highest and very similar capacity retention, in both cases higher than 98%. A2 shows slightly lower capacity retention, while A1 has much lower capacity retention, close to 80%, suggesting a more prominent presence of LAM and LLI within the cell.
The results show that the SOH measured during charging is consistently higher than during discharging for all batteries (F1, F2, A1, and A2). The CE values, listed in Table 5, indicate that F1, F2, and A1 have similar average CE values near 99%. In contrast, A2 has a lower CE of almost 95%. Typically, CE is characterized by three phases [23,40,41,42]. In the first cycles, there is a sharp increase in CE mainly due to the formation and growth of the solid electrolyte interphase (SEI). Afterward, the CE stabilizes around 100% and reaches the stable phase, which is maintained for hundreds of cycles. Finally, the third phase is characterized by a decrease in CE due to a sudden increase in chemical processes within the cell that cause LAM and LLI. The decreasing phase coincides with the capacity “knee” point [43]. Thus, CE is an indicator of the side reactions taking place within the battery [44]. In addition, it can give an indication of the capacity fade except when applied in the early stages; however, this is not a concern when considering second-life batteries that already have an aging history. From the obtained result, it emerges that A2, even if it has higher capacity retention than A1, may be more prone to degradation due to increased chemical side reactions occurring while electrochemically cycling. The different behavior can be attributed to the different aging paths followed by the two cells. This result indicates that A1 is in the stable phase like F1 and F2, while A2, due to the greater side reactions, might experience a more rapid decline in capacity retention after multiple cycles.
The charging and discharging times, used for measuring CCCT, CCDT, CVCT, and the ratio between CVCT and CCCT, are represented in Figure 7. The values for the aforementioned HIs are listed in Table 6.
The measured CCCT is similar for F1, F2, and A2 close to 6900 s, while it is lower for A1 with a value of 5760 s. On the other hand, the CCDT is lower for the electrically aged cells (A1, A2) compared to the non-electrically aged cells (F1, F2). The CCCT and CCDT decrease with aging [20,21,45,46], which is due to both IRI, which leads to an increase in the polarization of the cell upon charging [44], reaching higher voltages faster, and LAM, which contributes to reach the cell cut-off voltage faster [20,21]. From the results obtained, therefore, it can be assumed that A1 and A2 are characterized by higher LAM and IRI.
Similarly to CCCT, CVCT follows a similar trend, with higher values for F1, F2, and A2 compared to A1. The CVCT-based HI indicator bases its idea on the time required, which increases with aging due to the deceleration of charge transfer caused by the combination of the diffusion time slowdown, porosity changes, and electrolyte conductivity degradation over aging [22,45,47]. Contrary to what is expected, the CV-phase time is lower for the aged cell A1. This may be attributed to higher LLI than LAM for A1, resulting in reduced ions accumulation at the anode interface upon charging and allowing more effective intercalation in the active material.
Nonetheless, CVCT is sometimes considered an unreliable HI [21]. An alternative is to consider the percentage of time spent charging in CC compared to the total charging time. The ratio between CCCT and CVCT is lowest for F1 and highest for A2. However, in this case, the results do not appear to be directly related to aging, so no conclusions can be drawn about cell degradation.

3.2. Current–Time Behavior during the CV Charging Phase

The current trend over time during the CV phase is shown in Figure 8.
The approximating regression function, which contains coefficients a1 and a2, as well as the coefficient of determination, is based on Equation (3), and the obtained values are summarized in Table 7.
The results reveal that the coefficient a1 of the CVCP is higher for A1 and A2 compared to F1 and F2. On the other hand, the coefficient a2 is smaller for A1 compared to the other cells. As additional information, the coefficient of determination is higher for A1 compared to F1, F2, and A2.
As mentioned above, aging affects the CV phase [24]. In particular, the time spent during CV-charging increases with aging [22]. Thus by analyzing the CVCP, a steeper current decrease (higher coefficient a1 and lower coefficient a2) is expected for the non-electrically aged cells (F1, F2). The findings are in line with the CVCT findings, A1 has a higher coefficient a1, and a lower coefficient a2. This behavior can again be explained by a higher LLI than LAM for cell A1.

3.3. Voltage–Time Behavior at the End of Charging while Waiting-Voltage Relaxation Profile (VRP)

The voltage trend over time at the end of the charge is shown in Figure 9.
For each tested cell the voltage measured at the tabs after two hours and the voltage slope with respect to the time between the first and second hour are measured, and the obtained values are shown in Table 8.
From the VRP, it is shown that aged cells A1 and A2 relaxed to a lower voltage (below 4.17 V) value compared to cells F1 and F2 (above 4.17 V). A difference between A1 and A2 and F1 and F2 emerges also in the VRP slope and, in the last hour, the voltage of A1 and A2 drops faster compared to F1 and F2.
The VRP at the end of charging is correlated with aging. Aged cells’ voltage tends to relax to a lower voltage and requires more time to reach an equilibrium point [25,26]. The aging-related change in behavior is related to LLI and LAM, both of which reduce the amount of intercalable ions in the anode. In addition, LAM leads to a change in the crystal structure, which intrinsically affects the voltage measured at the battery electrodes [26,48]. Thus, considering the obtained results, worse behavior in both electrically aged cells A1 and A2 was found. Considering the results, both electrically aged cells A1 and A2 exhibit worse behavior, suggesting the presence of LAM and LLI as a degradation mechanism for both cells.

3.4. Voltage–Charge Behavior upon Cycling

The values of the area contained under the voltage–capacity curve during charging and discharging are shown in Figure 10.
The voltage–capacity curve area values are summarized in Table 9.
Similarly to the SOH, during aging there is a gradual shrinking of the area under the voltage–capacity curve. The shrinking of the area can be related to various degradation mechanisms and in particular to LLI and LAM [18]. During charging there is a lower value for A1, but similar values for F1, F2, and A2. During discharging, the values of A1 and A2 are lower than the values calculated for F1 and F2, suggesting LLI and LAM for the electrically aged cells.

3.5. Hysteresis Voltage Profile–Open Circuit Voltage (OCV) Approximation

The hysteresis OCV curves for all cells tested are shown in Figure 11.
The voltage values at 15 Ah, 25 Ah, and 35 Ah, as well as the slopes between 15 Ah and 25 Ah, and between 25 Ah and 35 Ah are considered as HIs, the measured values are shown in Table 10.
Generally, both at 35 Ah and 25 Ah and 15 Ah, cells A1 and A2 exhibit higher voltages than F1 and F2 for the same capacity. Additionally, both capacity–voltage slopes between the considered capacities are lower for A1 and A2 cells compared to F1 and F2.
For all five HIs extracted from the hysteresis OCV curve, a worse behavior for the electrically aged cells emerged. In general, the OCV curve is influenced by LAM, LLI, and IRI, thus it cannot be used to detect a specific degradation mechanism and it can be used to detect multiple degradation mechanisms [27], providing an overall idea of the aging state of the battery.

3.6. Thermal Evolution upon Cycling

The graphs in Figure 12 show the temperature evolution at different positions on the cell (i.e., near the negative tab and the positive tab) during charging and discharging. The absolute maximum temperature and the temperature rise are measured.
The thermal values measured during charging are shown in Table 11.
The maximum absolute temperatures on the negative tab ranged from 24.73 °C to 26.83 °C, with F2 exhibiting the highest temperature and F2 showing the lowest. On the positive tab, the maximum absolute temperatures during charging varied from 25.02 °C to 29.47 °C, with A2 displaying the highest value. The temperature rise on the negative tab upon charging was found to be in the range of 1.72 °C to 3.93 °C, with A2 experiencing the most significant temperature rise and F1 showing the smallest increase. On the positive tab, the temperature rise during charging ranged from 1.44 °C to 8.32 °C, again with A2 showing the highest temperature rise.
The thermal values measured during discharging are shown in Table 12.
The maximum absolute temperatures on the negative tab ranged from 24.57 °C to 28.04 °C, with F1 having the highest value and A2 having the lowest. On the positive tab, the maximum absolute temperatures during discharging varied from 25.93 °C to 27.47 °C, with A1 exhibiting the highest temperature. The temperature rise on the negative tab upon discharging was observed to be in the range of 2.67 °C to 4.13 °C, with F1 experiencing the highest temperature rise. On the positive tab, the temperature rise during discharging ranged from 2.97 °C to 4.13 °C, with Cell A2 demonstrating the highest temperature rise.
The temperature generated during charging or discharging, due to the ohmic effect, is correlated with the internal resistance of the battery [28,29,49,50]. Due to IRI, aged cells are expected to have a higher temperature rise. In general, cell A2 presented a worse thermal behavior with higher heat generation, which can be related to a greater IRI compared to the other cells.
The evolution of the temperature difference between the positive and negative tab during cell charging and discharging is shown in Figure 13.
The average and maximum temperature difference during charging and discharging are measured and listed in Table 13.
In general, higher values are observed on A2 than on F1, F2, and A1. Upon charging, the average temperature differences for the cells ranged from 0.37 °C (F2) to 1.87 °C (A2), while the maximum temperature differences varied from 0.41 °C (F2) to 1.30 °C (A2). Similarly, during discharging, the average temperature differences ranged from 0.55 °C (F2) to 4.47 °C (A2), with the maximum temperature differences ranging from 0.68 °C (F2) to 1.62 °C (A2). These findings indicate notable variations in the thermal behavior of the cells during charge and discharge cycles, with Cell A2 consistently displaying the most significant temperature differences, both in terms of average and maximum values. This behavior can be because aging leads to heterogeneous cell behavior [51]. At the thermal level, this is mainly related to IRI, which leads to increased heat generation [28,29,49,50] and to local lithium plating, i.e., LLI, which results in inhomogeneous current densities and thus inhomogeneous temperature distribution upon cycling [52,53].

3.7. Repeatability, Sensitivity, and Monotonicity Assessment

Once all absolute HI values have been extracted and/or calculated, Repeatability, Sensitivity, and Monotonicity are calculated. Table 14 summarizes the values for all the HIs considered in the analysis, with the Final score in the last column computed using Equation (11).
Comparing the Final score of the 31 HIs shows that some of them score higher than the others given considering Repeatability, Sensitivity, and Monotonicity scores. This allows a ranking to be made. All HIs that scored 12 or higher (upper-quartile) are considered to have good aging-sensitivity. All HIs between one and nine are considered to have lower aging-sensitivity and thus have less weight in the analysis. Finally, HIs with zero scores are not considered robust HIs and therefore are not considered in the analysis.
Additionally, the monotonicity criterion applied in this study played a crucial role in assessing the changes in HI values for aged cells compared to the non-electrically aged cells. The criterion ensured that the HIs exhibited consistent behavior in the same direction as the cells aged. Interestingly, when the monotonicity criterion was met, two distinct scenarios emerged: A1 exhibited worse behavior than A2 in some cases, while in other instances, the opposite trend was observed, with A2 showing more significant degradation than A1. These contrasting outcomes underscore the influence of different aging histories on the degradation mechanisms experienced by individual cells. It highlights that different degradation processes can be involved, depending on the unique aging conditions experienced by each cell. As a result, the identification of highly sensitive HIs that meet the monotonicity criterion offers a valuable tool to discern and spot the diverse degradation mechanisms that can occur in lithium-ion batteries during their operational lifetime.
Table 15 summarizes the HIs considered and their associated degradation mechanisms and the respective cell with the most critical score.
In summary, based on the experimental data of the HIs with scores greater than zero and on the monotonicity study, it can be concluded that cell A1 exhibits a predominant degradation mechanism of LLI, followed by LAM. On the other hand, for cell A2, the primary degradation mechanism is LAM, with IRI also playing a significant role.
This investigation’s limitations stem from the limited number of cells tested and the restriction to a single type per chemistry and shape.

4. Conclusions

Several HIs found in the scientific literature, which can be measured through standard onboard sensors during a basic charging–discharging cycle, were evaluated through a series of tests performed on 50 Ah commercial pouch cells. The aim was to obtain the most suitable HIs for qualifying second-life batteries considering their aging-sensitivity. The aging-sensitivity assessment was performed considering three criteria: repeatability, sensitivity, and monotonicity. The tests were conducted on four cells with different aging histories (F1, F2, A1, A2). In particular, two (A1 and A2) were electrically aged. The study showed that of the 31 HI:
  • Thirteen have good aging-sensitivity (i.e., SOH measured upon charging and discharging, the CE, the CCDT, the voltage trend extracted from the VRP, VdQ measured upon discharging, all the values extracted from the OCV curve, the maximum and average temperature difference between the tabs measured upon charging);
  • Six have poor aging-sensitivity (i.e., temperature rise measured on the positive tab upon charging, the relaxed voltage at the end of the VRP, the absolute peak temperature measured on the positive tab upon charging, a1 coefficient from the CVCP, R2 coefficient from the CVCP, and the temperature rise measured on the negative tab upon discharging);
  • Twelve failed to meet one of the criteria for sensitivity, repeatability, or monotonicity and thus are not suitable for battery qualification.
From the obtained results, it emerged that the behavior of some HIs differed when comparing the electrically aged cells, indicating that different aging histories can affect degradation phenomena differently within the cell. Specifically, cell A1 displayed a predominant degradation mechanism of LLI, followed by LAM, while A2 predominantly showed IRI and LAM. This highlights the need to consider multiple HIs for battery qualification, as different aging conditions may impact degradation differently.
The implications of these findings are significant for battery health monitoring systems, ensuring safe and efficient battery operation across various applications. By identifying and monitoring these sensitive HIs, more accurate assessments of battery aging and health can be achieved, enabling proactive maintenance and safety measures. Furthermore, the knowledge gained from this study is valuable for the evaluation of second-life batteries, assisting in the determination of their suitability for reuse and repurposing.
However, it is important to acknowledge that the study focused on aging-sensitivity, and the next step involves narrowing down the knowledge to address safety sensitivity specifically. Delving deeper into safety-related parameters during battery aging will facilitate the development of targeted safety assessment methodologies, further enhancing battery safety.

Author Contributions

Conceptualization, E.M., P.H. and J.M.; methodology, E.M., P.H. and J.M.; software, E.M.; validation, E.M.; formal analysis, E.M.; investigation, E.M.; resources, E.M.; data curation, E.M.; writing—original draft preparation, E.M.; writing—review and editing, E.M., P.H., S.M.A. and J.M.; visualization, E.M.; supervision, J.M.; project administration, C.E. and J.M.; funding acquisition, C.E. and J.M. All authors have read and agreed to the published version of the manuscript.

Funding

This work originates from the research project SafeLIB. The COMET Project SafeLIB is funded within the framework of COMET—Competence Centers for Excellent Technologies (Grant agreement No. 882506) by BMK, BMDW, the Province of Upper Austria, the province of Styria as well as SFG. The COMET Program is managed by FFG. The authors thank the consortium members of the SafeLIB project for supporting this work. Supported by the Open Access Funding by the Graz University of Technology.

Data Availability Statement

Not applicable.

Acknowledgments

Open Access Funding by the Graz University of Technology. The authors thank the consortium members of the SafeLIB project for their valuable input to this work.

Conflicts of Interest

The authors declare no conflict of interest.

Appendix A

Figure A1 illustrates the evaluation of the three criteria applied to the VRP data. For Repeatability, the spread of repeated cycle results on the same cell (F2_C3) is compared to the spread of cells with the same aging history (F2), and this criterion is used to validate the repeatability of the measurement. For Sensitivity, the spread of the non-electrically aged cells (F2) is compared to the spread of the entire dataset, and this criterion is used to ensure that there is a substantial difference between the non-electrically aged and electrically aged cells. Finally, Monotonicity is assessed by verifying that both electrically aged cells (A1 and A2) have changed in the same direction with respect to F1. In the shown example, the criterion is satisfied as both A1 and A2 are lower than F1, with A2 diverging further from F1 than A1. Thus, it emerged that A2’s aging has impacted the VRP relaxed voltage more than A1’s aging.
Figure A1. Illustrative example of the evaluation of the criteria used to rank the HIs applied to the VRP relaxed voltage results.
Figure A1. Illustrative example of the evaluation of the criteria used to rank the HIs applied to the VRP relaxed voltage results.
Batteries 09 00542 g0a1

References

  1. Garcia-Valle, R.; Peças Lopes, J.A. Electric Vehicle Integration into Modern Power Networks; Springer: New York, NY, USA; London, UK, 2013; ISBN 978-1-4614-0134-6. [Google Scholar]
  2. Olsson, L.; Fallahi, S.; Schnurr, M.; Diener, D.; van Loon, P. Circular Business Models for Extended EV Battery Life. Batteries 2018, 4, 57. [Google Scholar] [CrossRef]
  3. Hunt, G. US ABC Electric Vehicle Battery Test Procedures Manual, Revision 2; DOE/ID-10479; Idaho National Engineering Laboratory (INEL), US Department of Energy Idaho Field Office: Washington, DC, USA, 1996; Volume 2, p. 39. [Google Scholar]
  4. Michelini, E.; Höschele, P.; Ratz, F.; Stadlbauer, M.; Rom, W.; Ellersdorfer, C.; Moser, J. Potential and Most Promising Second-Life Applications for Automotive Lithium-Ion Batteries Considering Technical, Economic and Legal Aspects. Energies 2023, 16, 2830. [Google Scholar] [CrossRef]
  5. Han, X.; Ouyang, M.; Lu, L.; Li, J.; Zheng, Y.; Li, Z. A comparative study of commercial lithium ion battery cycle life in electrical vehicle: Aging mechanism identification. J. Power Sources 2014, 251, 38–54. [Google Scholar] [CrossRef]
  6. Gao, Y.; Jiang, J.; Zhang, C.; Zhang, W.; Jiang, Y. Aging mechanisms under different state-of-charge ranges and the multi-indicators system of state-of-health for lithium-ion battery with Li(NiMnCo)O2 cathode. J. Power Sources 2018, 400, 641–651. [Google Scholar] [CrossRef]
  7. Vetter, J.; Novák, P.; Wagner, M.R.; Veit, C.; Möller, K.-C.; Besenhard, J.O.; Winter, M.; Wohlfahrt-Mehrens, M.; Vogler, C.; Hammouche, A. Ageing mechanisms in lithium-ion batteries. J. Power Sources 2005, 147, 269–281. [Google Scholar] [CrossRef]
  8. Birkl, C.R.; Roberts, M.R.; McTurk, E.; Bruce, P.G.; Howey, D.A. Degradation diagnostics for lithium ion cells. J. Power Sources 2017, 341, 373–386. [Google Scholar] [CrossRef]
  9. Xiong, R.; Pan, Y.; Shen, W.; Li, H.; Sun, F. Lithium-ion battery aging mechanisms and diagnosis method for automotive applications: Recent advances and perspectives. Renew. Sustain. Energy Rev. 2020, 131, 110048. [Google Scholar] [CrossRef]
  10. Abada, S.; Petit, M.; Lecocq, A.; Marlair, G.; Sauvant-Moynot, V.; Huet, F. Combined experimental and modeling approaches of the thermal runaway of fresh and aged lithium-ion batteries. J. Power Sources 2018, 399, 264–273. [Google Scholar] [CrossRef]
  11. Xie, S.; Ren, L.; Yang, X.; Wang, H.; Sun, Q.; Chen, X.; He, Y. Influence of cycling aging and ambient pressure on the thermal safety features of lithium-ion battery. J. Power Sources 2020, 448, 227425. [Google Scholar] [CrossRef]
  12. Preger, Y.; Torres-Castro, L.; Rauhala, T.; Jeevarajan, J. Perspective—On the Safety of Aged Lithium-Ion Batteries. J. Electrochem. Soc. 2022, 169, 30507. [Google Scholar] [CrossRef]
  13. Schmidt, A.; Smith, A.; Ehrenberg, H. Power capability and cyclic aging of commercial, high power lithium ion battery cells with respect to different cell designs. J. Power Sources 2019, 425, 27–38. [Google Scholar] [CrossRef]
  14. Han, X.; Lu, L.; Zheng, Y.; Feng, X.; Li, Z.; Li, J.; Ouyang, M. A review on the key issues of the lithium ion battery degradation among the whole life cycle. eTransportation 2019, 1, 100005. [Google Scholar] [CrossRef]
  15. Rufino Júnior, C.A.; Sanseverino, E.R.; Gallo, P.; Koch, D.; Kotak, Y.; Schweiger, H.-G.; Zanin, H. Reviewing Regulations and Standards for Second-Life Batteries. Preprints 2023, 2023060711. [Google Scholar] [CrossRef]
  16. Zhou, W.; Lu, Q.; Zheng, Y. Review on the Selection of Health Indicator for Lithium Ion Batteries. Machines 2022, 10, 512. [Google Scholar] [CrossRef]
  17. Dubarry, M.; Truchot, C.; Liaw, B.Y. Synthesize battery degradation modes via a diagnostic and prognostic model. J. Power Sources 2012, 219, 204–216. [Google Scholar] [CrossRef]
  18. Xiong, W.; Xu, G.; Li, Y.; Zhang, F.; Ye, P.; Li, B. Early prediction of lithium-ion battery cycle life based on voltage-capacity discharge curves. J. Energy Storage 2023, 62, 106790. [Google Scholar] [CrossRef]
  19. Anseán, D.; Dubarry, M.; Devie, A.; Liaw, B.Y.; García, V.M.; Viera, J.C.; González, M. Fast charging technique for high power LiFePO4 batteries: A mechanistic analysis of aging. J. Power Sources 2016, 321, 201–209. [Google Scholar] [CrossRef]
  20. Wei, M.; Gu, H.; Ye, M.; Wang, Q.; Xu, X.; Wu, C. Remaining useful life prediction of lithium-ion batteries based on Monte Carlo Dropout and gated recurrent unit. Energy Rep. 2021, 7, 2862–2871. [Google Scholar] [CrossRef]
  21. Sun, Y.; Hao, X.; Pecht, M.; Zhou, Y. Remaining useful life prediction for lithium-ion batteries based on an integrated health indicator. Microelectron. Reliab. 2018, 88–90, 1189–1194. [Google Scholar] [CrossRef]
  22. Eddahech, A.; Briat, O.; Vinassa, J.-M. Determination of lithium-ion battery state-of-health based on constant-voltage charge phase. J. Power Sources 2014, 258, 218–227. [Google Scholar] [CrossRef]
  23. Yang, F.; Wang, D.; Zhao, Y.; Tsui, K.-L.; Bae, S.J. A study of the relationship between coulombic efficiency and capacity degradation of commercial lithium-ion batteries. Energy 2018, 145, 486–495. [Google Scholar] [CrossRef]
  24. Wang, R.; Feng, H. Remaining useful life prediction of lithium-ion battery using a novel health indicator. Qual. Reliab. Engng. Int. 2021, 37, 1232–1243. [Google Scholar] [CrossRef]
  25. Tseng, K.-H.; Liang, J.-W.; Chang, W.; Huang, S.-C. Regression Models Using Fully Discharged Voltage and Internal Resistance for State of Health Estimation of Lithium-Ion Batteries. Energies 2015, 8, 2889–2907. [Google Scholar] [CrossRef]
  26. Baghdadi, I.; Briat, O.; Gyan, P.; Vinassa, J.M. State of health assessment for lithium batteries based on voltage–time relaxation measure. Electrochim. Acta 2016, 194, 461–472. [Google Scholar] [CrossRef]
  27. Schmidt, J.P.; Tran, H.Y.; Richter, J.; Ivers-Tiffée, E.; Wohlfahrt-Mehrens, M. Analysis and prediction of the open circuit potential of lithium-ion cells. J. Power Sources 2013, 239, 696–704. [Google Scholar] [CrossRef]
  28. Menale, C.; D’Annibale, F.; Mazzarotta, B.; Bubbico, R. Thermal management of lithium-ion batteries: An experimental investigation. Energy 2019, 182, 57–71. [Google Scholar] [CrossRef]
  29. Waldmann, T.; Wilka, M.; Kasper, M.; Fleischhammer, M.; Wohlfahrt-Mehrens, M. Temperature dependent ageing mechanisms in Lithium-ion batteries—A Post-Mortem study. J. Power Sources 2014, 262, 129–135. [Google Scholar] [CrossRef]
  30. Xiong, R.; He, H.; Sun, F.; Zhao, K. Evaluation on State of Charge Estimation of Batteries with Adaptive Extended Kalman Filter by Experiment Approach. IEEE Trans. Veh. Technol. 2013, 62, 108–117. [Google Scholar] [CrossRef]
  31. Zhang, S.S. A review on the separators of liquid electrolyte Li-ion batteries. J. Power Sources 2007, 164, 351–364. [Google Scholar] [CrossRef]
  32. Ng, K.S.; Moo, C.-S.; Chen, Y.-P.; Hsieh, Y.-C. Enhanced coulomb counting method for estimating state-of-charge and state-of-health of lithium-ion batteries. Appl. Energy 2009, 86, 1506–1511. [Google Scholar] [CrossRef]
  33. Tong, S.; Klein, M.P.; Park, J.W. On-line optimization of battery open circuit voltage for improved state-of-charge and state-of-health estimation. J. Power Sources 2015, 293, 416–428. [Google Scholar] [CrossRef]
  34. Weng, C.; Sun, J.; Peng, H. A unified open-circuit-voltage model of lithium-ion batteries for state-of-charge estimation and state-of-health monitoring. J. Power Sources 2014, 258, 228–237. [Google Scholar] [CrossRef]
  35. Xing, Y.; He, W.; Pecht, M.; Tsui, K.L. State of charge estimation of lithium-ion batteries using the open-circuit voltage at various ambient temperatures. Appl. Energy 2014, 113, 106–115. [Google Scholar] [CrossRef]
  36. Plett, G.L. Extended Kalman filtering for battery management systems of LiPB-based HEV battery packs. J. Power Sources 2004, 134, 277–292. [Google Scholar] [CrossRef]
  37. Dreyer, W.; Jamnik, J.; Guhlke, C.; Huth, R.; Moskon, J.; Gaberscek, M. The thermodynamic origin of hysteresis in insertion batteries. Nat. Mater. 2010, 9, 448–453. [Google Scholar] [CrossRef]
  38. Chen, X.; Hu, Y.; Li, S.; Wang, Y.; Li, D.; Luo, C.; Xue, X.; Xu, F.; Zhang, Z.; Gong, Z.; et al. State of health (SoH) estimation and degradation modes analysis of pouch NMC532/graphite Li-ion battery. J. Power Sources 2021, 498, 229884. [Google Scholar] [CrossRef]
  39. Li, J.; Adewuyi, K.; Lotfi, N.; Landers, R.G.; Park, J. A single particle model with chemical/mechanical degradation physics for lithium ion battery State of Health (SOH) estimation. Appl. Energy 2018, 212, 1178–1190. [Google Scholar] [CrossRef]
  40. Gyenes, B.; Stevens, D.A.; Chevrier, V.L.; Dahn, J.R. Understanding Anomalous Behavior in Coulombic Efficiency Measurements on Li-Ion Batteries. J. Electrochem. Soc. 2014, 162, A278–A283. [Google Scholar] [CrossRef]
  41. Deshpande, R.D.; Ridgway, P.; Fu, Y.; Zhang, W.; Cai, J.; Battaglia, V. The Limited Effect of VC in Graphite/NMC Cells. J. Electrochem. Soc. 2014, 162, A330–A338. [Google Scholar] [CrossRef]
  42. Xu, J.; Deshpande, R.D.; Pan, J.; Cheng, Y.-T.; Battaglia, V.S. Electrode Side Reactions, Capacity Loss and Mechanical Degradation in Lithium-Ion Batteries. J. Electrochem. Soc. 2015, 162, A2026–A2035. [Google Scholar] [CrossRef]
  43. Diao, W.; Saxena, S.; Han, B.; Pecht, M. Algorithm to Determine the Knee Point on Capacity Fade Curves of Lithium-Ion Cells. Energies 2019, 12, 2910. [Google Scholar] [CrossRef]
  44. Saha, B.; Goebel, K. Modeling Li-ion Battery Capacity Depletion in a Particle Filtering Framework. In Proceedings of the Annual Conference of the PHM Society, Virtual, 29 November–2 December 2021. [Google Scholar]
  45. Williard, N.; He, W.; Osterman, M.; Pecht, M. Comparative Analysis of Features for Determining State of Health in Lithium-Ion Batteries. IJPHM 2013, 4. [Google Scholar] [CrossRef]
  46. Yun, Z.; Qin, W. Remaining Useful Life Estimation of Lithium-Ion Batteries Based on Optimal Time Series Health Indicator. IEEE Access 2020, 8, 55447–55461. [Google Scholar] [CrossRef]
  47. Ruan, H.; He, H.; Wei, Z.; Quan, Z.; Li, Y. State of Health Estimation of Lithium-ion Battery Based on Constant-Voltage Charging Reconstruction. IEEE J. Emerg. Sel. Top. Power Electron. 2021, 11, 4393–4402. [Google Scholar] [CrossRef]
  48. Tarascon, J.M.; Armand, M. Issues and challenges facing rechargeable lithium batteries. Nature 2001, 414, 359–367. [Google Scholar] [CrossRef] [PubMed]
  49. Bodenes, L.; Naturel, R.; Martinez, H.; Dedryvère, R.; Menetrier, M.; Croguennec, L.; Pérès, J.-P.; Tessier, C.; Fischer, F. Lithium secondary batteries working at very high temperature: Capacity fade and understanding of aging mechanisms. J. Power Sources 2013, 236, 265–275. [Google Scholar] [CrossRef]
  50. Stiaszny, B.; Ziegler, J.C.; Krauß, E.E.; Schmidt, J.P.; Ivers-Tiffée, E. Electrochemical characterization and post-mortem analysis of aged LiMn2O4–Li(Ni0.5Mn0.3Co0.2)O2/graphite lithium ion batteries. Part I: Cycle aging. J. Power Sources 2014, 251, 439–450. [Google Scholar] [CrossRef]
  51. Michelini, E.; Höschele, P.; Heindl, S.F.; Erker, S.; Ellersdorfer, C. Experimental Investigation on Reversible Swelling Mechanisms of Lithium-Ion Batteries under a Varying Preload Force. Batteries 2023, 9, 218. [Google Scholar] [CrossRef]
  52. Choudhari, V.G.; Dhoble, A.S.; Sathe, T.M. A review on effect of heat generation and various thermal management systems for lithium ion battery used for electric vehicle. J. Energy Storage 2020, 32, 101729. [Google Scholar] [CrossRef]
  53. Xie, Y.; Wang, S.; Li, R.; Ren, D.; Yi, M.; Xu, C.; Han, X.; Lu, L.; Friess, B.; Offer, G.; et al. Inhomogeneous degradation induced by lithium plating in a large-format lithium-ion battery. J. Power Sources 2022, 542, 231753. [Google Scholar] [CrossRef]
Figure 1. Voltage–time curve upon (a) charging and (b) discharging with extracted HIs.
Figure 1. Voltage–time curve upon (a) charging and (b) discharging with extracted HIs.
Batteries 09 00542 g001
Figure 2. Current–time during CV reference curve. The red line refers to the real data and the black line to the exponential regression function.
Figure 2. Current–time during CV reference curve. The red line refers to the real data and the black line to the exponential regression function.
Batteries 09 00542 g002
Figure 3. VRP from which the relaxed voltage and the voltage slope HIs are extracted.
Figure 3. VRP from which the relaxed voltage and the voltage slope HIs are extracted.
Batteries 09 00542 g003
Figure 4. Voltage−charge curves during (a) charging and (b) discharging with the extracted HIs.
Figure 4. Voltage−charge curves during (a) charging and (b) discharging with the extracted HIs.
Batteries 09 00542 g004
Figure 5. Hysteresis OCV: charging and discharging curve, averaged curve, and HIs extracted.
Figure 5. Hysteresis OCV: charging and discharging curve, averaged curve, and HIs extracted.
Batteries 09 00542 g005
Figure 6. Thermal evolution on the cell. The exemplary thermal rise Trise in this case is referred to the negative tab, a similar procedure is followed for the positive tab.
Figure 6. Thermal evolution on the cell. The exemplary thermal rise Trise in this case is referred to the negative tab, a similar procedure is followed for the positive tab.
Batteries 09 00542 g006
Figure 7. Voltage–time curves during (a) charging and (b) discharging.
Figure 7. Voltage–time curves during (a) charging and (b) discharging.
Batteries 09 00542 g007
Figure 8. Current–time curve at the end of the CC charging, during the CV phase.
Figure 8. Current–time curve at the end of the CC charging, during the CV phase.
Batteries 09 00542 g008
Figure 9. Voltage trends over time (i.e., VRP) at the end of the CC-CV charge.
Figure 9. Voltage trends over time (i.e., VRP) at the end of the CC-CV charge.
Batteries 09 00542 g009
Figure 10. Voltage−charge curves during (a) charging and (b) discharging.
Figure 10. Voltage−charge curves during (a) charging and (b) discharging.
Batteries 09 00542 g010
Figure 11. Hysteresis voltage profile results.
Figure 11. Hysteresis voltage profile results.
Batteries 09 00542 g011
Figure 12. Temperature evolution during charging (a) and discharging (b) measured close to the negative tab and during charging (c) and discharging (d) measured close to the positive tab.
Figure 12. Temperature evolution during charging (a) and discharging (b) measured close to the negative tab and during charging (c) and discharging (d) measured close to the positive tab.
Batteries 09 00542 g012
Figure 13. Temperature difference during charging (a) and discharging (b) between the measurement taken close to the negative tab and the positive tab.
Figure 13. Temperature difference during charging (a) and discharging (b) between the measurement taken close to the negative tab and the positive tab.
Batteries 09 00542 g013
Table 1. List of considered HIs.
Table 1. List of considered HIs.
Reference CurveHealth IndicatorDescription
Voltage–time behavior upon charging
[20,21,22]
State of Health (SOH) upon chargingRatio of the remaining useful capacity over the nominal capacity
Constant current charge time (CCCT)Time needed by the battery to reach the CV phase upon charging
Constant voltage charge time (CVCT)Time spent by the battery in the CV phase upon charging
Ratio CVCT/CCCTRatio between CVCT and CCCT
Voltage–time behavior upon discharging
[20,21,23]
State of health (SOH) upon dischargingRatio of the remaining useful capacity over the nominal capacity
Coulomb efficiency (CE)Ratio of the charged over the discharged capacity
Constant current discharge time (CCDT)Time spent by the battery in the CC phase upon discharging
Current–time behavior during the CV charging phase
[24]
Constant voltage current profile (CVCP)–a1Coefficients a1 of the CVCP profile, see Equation (3)
Constant voltage current profile (CVCP)–a2Coefficients a2 of the CVCP profile, see Equation (3)
Constant voltage current profile (CVCP)–R2Coefficient of determination of the CVCP profile, see Equation (3)
Voltage–time behavior at the end of charging while waiting
[25,26]
Voltage relaxation profile (VRP)–relaxed voltageVoltage measured after a 2 h waiting time after charging
Voltage relaxation profile (VRP)–slopeRate of voltage decrease over time during the last hour of waiting time
Voltage–charge behavior upon cycling
[18,27,30]
Area VdQ chargingIntegral of the voltage over the charge
Area VdQ dischargingIntegral of the voltage over the charge
OCV at 15 AhVoltage measured at 15 Ah considering the hysteresis OCV curve
OCV at 25 AhVoltage measured at 25 Ah considering the hysteresis OCV curve
OCV at 35 AhVoltage measured at 35 Ah considering the hysteresis OCV curve
OCV slope between 15–25 AhRate of voltage change over the charge between 15 and 25 Ah in the hysteresis OCV curve
OCV slope between 25–35 AhRate of voltage change over the charge between 25 and 35 Ah in the hysteresis OCV curve
Thermal evolution upon charging and discharging
[28,29]
Max T negative tabHighest absolute temperature recorded on the negative tab
Max T positive tabHighest absolute temperature recorded on the positive tab
T rise negative tabMaximum absolute temperature minus the minimum absolute temperature measured on the negative tab
T rise positive tabMaximum absolute temperature minus the minimum absolute temperature measured on the positive tab
Average T differenceAverage temperature difference measured between the tabs of the cell
Maximum T differenceMaximum temperature difference measured between the tabs of the cell
Table 2. Aging history of tested cells.
Table 2. Aging history of tested cells.
Aging HistoryCalendar AgingCycling TimeAverage TemperatureTemperature RangeAverage Charging CurrentMax Charging CurrentAvg Discharging CurrentMax Discharging Current
[Years][h][°C][°C][A][A][A][A]
F1702710–3538>5019<−150
F210820−40–4510>5075<−150
A181239210–4036>5017<−150
A276132710–3538>5019<−150
Table 3. Corresponding Repeatability and Sensitivity scores.
Table 3. Corresponding Repeatability and Sensitivity scores.
ValueEvaluation Scoring
Repeatability/Sensitivity < 0.254
0.25 ≤ Repeatability/Sensitivity < 0.503
0.50 ≤ Repeatability/Sensitivity < 0.752
0.75 ≤ Repeatability/Sensitivity < 1.001
Repeatability/Sensitivity > 1.000
Table 4. Corresponding Monotonicity scores.
Table 4. Corresponding Monotonicity scores.
ValueEvaluation Scoring
Monotonicity > 01
Monotonicity < 00
Table 5. Absolute values obtained through the different tests of the HIs: SOH charging, SOH discharging, and Coulombic efficiency.
Table 5. Absolute values obtained through the different tests of the HIs: SOH charging, SOH discharging, and Coulombic efficiency.
Cell IDSOH Charging [%]SOH Discharging [%]Coulombic Efficiency [%]
CellAverageCellAverageCellAverage
F199.7099.7099.1999.1999.4899.48
F2_C198.3699.2898.2798.2799.9098.99
F2_C298.1797.2899.09
F2_C399.8498.5498.70
99.9298.4898.56
100.1098.8198.71
A181.0081.0080.0380.0398.8098.80
A297.5397.5392.9092.9095.2695.26
Table 6. Absolute values obtained through the different tests of the HIs: CCCT, CVCT, CVCT/CCCT, and CCDT.
Table 6. Absolute values obtained through the different tests of the HIs: CCCT, CVCT, CVCT/CCCT, and CCDT.
Cell IDCCCT [s]CVCT [s] C V C T C C C T [%]CCDT [s]
CellAverageCellAverageCellAverageCellAverage
F1689968991285128518.6318.6373137313
F2_C1681968501206132417.6919.3272457246
F2_C26775129219.077172
F2_C36870139120.257265
6864143320.877262
6924129718.747286
A1576057601081108118.7718.7760716071
A2692069201363136319.6919.6970467046
Table 7. Absolute values obtained through the different tests of the CVCP HIs.
Table 7. Absolute values obtained through the different tests of the CVCP HIs.
Cell IDa1a2 [×103]Coefficient of Determination [%]
CellAverageCellAverageCellAverage
F122.4922.49−1.83837−1.8499.5799.57
F2_C122.8122.57−1.94976−1.7899.7399.64
F2_C222.49−1.8238199.60
F2_C322.49−1.6878499.63
22.51−1.6491599.60
22.54−1.8133599.63
A122.8322.83−2.21677−2.2299.6999.69
A222.7522.75−1.77636−1.7899.6099.60
Table 8. Absolute values obtained through the different tests of the VRP His.
Table 8. Absolute values obtained through the different tests of the VRP His.
Cell IDRelaxed Voltage [V]Voltage Trend [V × 10−6/s]
CellAverageCellAverage
F14.1764.176−0.040−0.040
F2_C14.1784.175−0.032−0.040
F2_C24.174−0.051
F2_C34.175−0.042
4.175−0.039
4.176−0.039
A14.1684.168−0.165−0.165
A24.1634.163−0.213−0.213
Table 9. Absolute values obtained through the different tests of the voltage–capacity curve area upon charging and upon discharging.
Table 9. Absolute values obtained through the different tests of the voltage–capacity curve area upon charging and upon discharging.
Cell IDVoltage–Capacity Curve Area upon Charging [VAh]Voltage–Capacity Curve Area upon Discharging [VAh]
CellAverageCellAverage
F1196.47196.47185.06185.06
F2_C1194.00195.71183.36183.05
F2_C2193.32181.25
F2_C3197.00183.39
197.11183.18
197.13184.05
A1165.03165.03154.44154.44
A2198.84198.84177.44177.44
Table 10. Absolute values obtained through the different tests of hysteresis OCV curve HIs.
Table 10. Absolute values obtained through the different tests of hysteresis OCV curve HIs.
Cell IDVoltage (35 Ah) [V]Voltage (25 Ah) [V]Voltage (15 Ah) [V]Voltage Change (35–25 Ah) [Ah/V]Voltage Change (25–15 Ah) [Ah/V]
CellAverageCellAverageCellAverageCellAverageCellAverage
F13.813.813.683.683.603.6075.2975.29117.73117.73
F2_C13.823.823.683.683.603.5972.4473.36115.67115.05
F2_C23.833.693.5970.25109.74
F2_C33.813.683.5974.77116.69
3.813.683.5974.40115.95
3.813.683.5974.93117.19
A13.983.983.783.783.643.6450.3750.3772.5472.54
A23.833.833.693.693.603.6068.6268.62110.05110.05
Table 11. Absolute values obtained through the different tests of the following thermal HIs: maximum absolute temperature on the positive and negative tab upon charging and discharging.
Table 11. Absolute values obtained through the different tests of the following thermal HIs: maximum absolute temperature on the positive and negative tab upon charging and discharging.
Cell IDMax T Negative Tab upon Charging [°C]Max T Negative Tab upon Discharging [°C]Max T Positive Tab upon Charging [°C]Max T Positive Tab upon Discharging [°C]
CellAverageCellAverageCellAverageCellAverage
F126.8326.8328.0428.0426.1826.1827.0427.04
F2_C127.2224.7329.0925.6327.0725.0228.8025.93
F2_C225.8026.5925.5426.17
F2_C323.4424.1424.0424.91
22.9223.8523.5724.60
24.2724.4724.8825.17
A125.7925.7926.6426.6426.7326.7327.4727.47
A225.1525.1524.5724.5729.4729.4726.0126.01
Table 12. Absolute values obtained through the different tests of the following thermal HIs: absolute temperature rise on the positive and negative tab upon charging and discharging.
Table 12. Absolute values obtained through the different tests of the following thermal HIs: absolute temperature rise on the positive and negative tab upon charging and discharging.
Cell IDT Rise Negative Tab upon Charging [°C]T Rise Negative Tab upon Discharging [°C]T Rise Positive Tab upon Charging [°C]T Rise Positive Tab upon Discharging [°C]
CellAverageCellAverageCellAverageCellAverage
F11.841.844.134.131.441.443.243.24
F2_C12.532.253.913.312.562.673.713.70
F2_C21.122.681.032.39
F2_C32.283.302.984.16
2.323.553.064.38
2.983.103.703.88
A11.721.722.672.672.612.612.972.97
A23.933.932.842.848.328.324.134.13
Table 13. Absolute values obtained through the different tests of the following thermal HIs: average and maximum temperature difference between tabs upon charging and discharging.
Table 13. Absolute values obtained through the different tests of the following thermal HIs: average and maximum temperature difference between tabs upon charging and discharging.
Cell IDAverage T Difference upon Charging [°C]Average T Difference upon Discharging [°C]Maximum T Difference upon Charging [°C]Maximum T Difference upon Discharging [°C]
CellAverageCellAverageCellAverageCellAverage
F10.560.560.740.740.870.871.191.19
F2_C10.180.370.270.550.210.410.390.68
F2_C20.220.300.290.49
F2_C30.470.710.510.85
0.500.740.520.82
0.480.740.510.86
A10.600.601.021.020.750.750.900.90
A21.871.874.474.471.301.301.621.62
Table 14. Repeatability, Sensitivity, and Monotonicity values and final score for the investigated HIs.
Table 14. Repeatability, Sensitivity, and Monotonicity values and final score for the investigated HIs.
Health IndicatorRepeatabilitySensitivityMonotonicityFinal Score
ValueScoreValueScoreValueScore
SOH charging0.1340.1444.10 × 101116
OCV–35 Ah0.2240.1343.20 × 10−3116
OCV–Slope (15−25 Ah)0.1940.1943.50 × 102116
OCV–Slope (25−35 Ah)0.1240.2341.70 × 102116
Max T difference charging0.0740.1741.10 × 100116
SOH discharging0.2730.0941.20 × 102112
Coulombic efficiency0.1440.3732.90 × 100112
CCDT0.2730.1043.30 × 105112
VdQ discharging0.3930.1042.30 × 102112
VRP–V trend0.2730.0942.20 × 10−2112
OCV–15 Ah0.4730.1844.70 × 10−5112
OCV–25 Ah0.3630.1246.80 × 10−4112
Average T difference charging0.1040.2835.70 × 10−2112
VRP–Relaxed V0.4730.2831.20 × 10−419
T rise positive tab charging0.3630.4338.10 × 10019
Peak T positive tab charging0.4430.7021.80 × 10016
CVCP–a10.1640.8519.00 × 10−214
CVCP–R20.3030.9414.80 × 10−713
T rise negative tab discharging0.4530.8011.90 × 10013
CCCT0.5320.144−2.40 × 10400
CVCT0.7120.771−1.60 × 10400
CVCT/CCCT0.8011.1901.60 × 10−110
CVCP–a20.6520.652−2.30 × 10−800
VdQ charging0.0340.164−7.40 × 10100
Peak T negative tab charging0.3531.1001.80 × 10010
Peak T negative tab discharging0.1341.0804.80 × 10010
Peak T positive tab discharging0.1541.140−4.50 × 10−100
T rise negative tab charging0.5220.771−2.70 × 10−100
T rise positive tab discharging0.2931.090−2.30 × 10−100
Average T difference discharging0.0240.403−5.20 × 10−200
Max T difference discharging0.0940.562−1.20 × 10−100
Table 15. Aging-sensitive HI list with corresponding degradation mechanism and the electrically aged cell where it has shown worse behavior.
Table 15. Aging-sensitive HI list with corresponding degradation mechanism and the electrically aged cell where it has shown worse behavior.
Health IndicatorMain Degradation MechanismElectrically Aged Cell
SOH chargingLAM, LLIA1
OCV–35 AhLAM, LLIA1
OCV–Slope (15–25 Ah)LAM, LLI, IRIA1
OCV–Slope (25–35 Ah)LAM, LLI, IRIA1
Max T difference chargingLLI, IRIA2
SOH dischargingLAM, IRIA1
Coulombic efficiencyLAM, LLIA2
CCDTLAM, LLIA1
VdQ dischargingLAM, LLIA1
VRP–V trendLAMA2
OCV–15 AhLAM, LLI, IRIA1
OCV–25 AhLAM, LLI, IRIA1
Average T difference chargingLLI, IRIA2
VRP–Relaxed VLAMA2
T rise positive tab chargingIRIA1
Peak T positive tab chargingIRIA1
CVCP–a1LLIA1
CVCP–R2-A1
T rise negative tab dischargingIRIA2
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content.

Share and Cite

MDPI and ACS Style

Michelini, E.; Höschele, P.; Abbas, S.M.; Ellersdorfer, C.; Moser, J. Assessment of Health Indicators to Detect the Aging State of Commercial Second-Life Lithium-Ion Battery Cells through Basic Electrochemical Cycling. Batteries 2023, 9, 542. https://doi.org/10.3390/batteries9110542

AMA Style

Michelini E, Höschele P, Abbas SM, Ellersdorfer C, Moser J. Assessment of Health Indicators to Detect the Aging State of Commercial Second-Life Lithium-Ion Battery Cells through Basic Electrochemical Cycling. Batteries. 2023; 9(11):542. https://doi.org/10.3390/batteries9110542

Chicago/Turabian Style

Michelini, Emanuele, Patrick Höschele, Syed Muhammad Abbas, Christian Ellersdorfer, and Jörg Moser. 2023. "Assessment of Health Indicators to Detect the Aging State of Commercial Second-Life Lithium-Ion Battery Cells through Basic Electrochemical Cycling" Batteries 9, no. 11: 542. https://doi.org/10.3390/batteries9110542

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.

Article Metrics

Back to TopTop