Next Article in Journal
Mineralogy of Phoscorites of the Arbarastakh Complex (Republic of Sakha, Yakutia, Russia)
Next Article in Special Issue
Elimination of Ferric Ion Effect on Separation between Kyanite and Quartz Using Citric Acid as Regulator
Previous Article in Journal
Stability of Atrazine–Smectite Intercalates: Density Functional Theory and Experimental Study
Previous Article in Special Issue
Adsorption Behaviors of Straight-Chain Alkanes on a Molybdenite [001]/[100] Surface: A Molecular Dynamics Study
 
 
Font Type:
Arial Georgia Verdana
Font Size:
Aa Aa Aa
Line Spacing:
Column Width:
Background:
Article

Clean and Feasible Utilization of High Silica Fluorspar Powder via Reverse Flotation: A Pilot Study

1
School of Chemistry and Material engineering, Liupanshui Normal University, Liupanshui 553004, China
2
School of Mineral Processing and Bioengineering, Central South University, Changsha 410083, China
3
College of Chemistry and Chemical Engineering, Central South University, Changsha 410083, China
*
Author to whom correspondence should be addressed.
Minerals 2021, 11(6), 555; https://doi.org/10.3390/min11060555
Submission received: 16 April 2021 / Revised: 19 May 2021 / Accepted: 20 May 2021 / Published: 24 May 2021
(This article belongs to the Special Issue Flotation Chemistry, Volume II)

Abstract

:
Fluorite is a nonrenewable mineral used to produce anhydrous hydrofluoric acid (AHF) and aluminum fluoride. The demand for low-grade fluorite powder (CaF2 < 97%) has fallen sharply owing to the current market conditions. Therefore, a large number of fluorite concentrates have been improved by acid leaching. While this approach can efficiently remove CaCO3 from fluorite concentrate, the SiO2 content, which significantly affects AHF consumption during the production of HF or aluminum fluoride, cannot be completely removed. To solve this problem, in this study, we used reverse flotation before leaching the fluorite concentrates. Subsequently, the feasibility of reverse flotation desilication was determined. The obtained results of the ZP (zeta potential) measurements, solution chemistry analysis, FTIR (Fourier transform infrared spectroscopy) analysis, and micro-flotation tests indicated that employing dodecylamine as the collector and citric acid as the depressor could effectively separate sericite from fluorite. The batch flotation experiment and the pilot test were conducted in Chenzhou (Hunan, China) followed by their operation in Xinyuan Mining Co. Ltd., which produces monolithic fluorite ore on the large scale in Asia. Notably, we found that the contents of both SiO2 and Al2O3 were from 2.82%, 1.17% reduced to 1.28%, 0.74% in the batch flotation experiment. The results of the pilot test showed that the new reverse flotation + leaching technology could dramatically reduce the potential environmental impact and costs, thereby significantly improving the economic benefits by satisfying the requirements of the market.

Graphical Abstract

1. Introduction

Fluorite (CaF2) is a non-renewable mineral and is employed as a flux agent in steelmaking and hydrofluoric acid production [1,2]. In China, the mineral is derived mainly from naturally occurring fluorite minerals and tailings of tungsten, and there are a few notable differences between both the production processes. Moreover, the ultimate objective of every Chinese company is to produce high-grade products (CaF2 ≥ 97%, SiO2 < 1%).
In the past, the fluorite concentrate’s quality index was usually CaF2 ≥ 97%. However, although the fluorite production was efficient, the side effects of resource exploitation in China were becoming increasingly apparent, and it was difficult to maintain a steady production of high-grade fluorite, which contained more impurities than before. The two major impurities found in fluorite concentrates are carbonate (CaCO3) and silicate (SiO2). Several studies reported that all commercial fluorite production processes used froth flotation to remove the impurities [3,4,5,6,7]. Furthermore, this method was widely employed to remove gangue minerals from fluorite concentrations to further improve the fluorite grade [8,9,10,11].
The Jiepailing fluorite mine is the single largest fluorite deposit in China, and has the largest ore of monolithic fluorite in Asia, and reserves 26.21 million tons of CaF2 mineral. In our previous study, the use of a two-stage depressed technology in the Jiepailing fluorite mine proved to be successful [12]. Thus far, a two-stage depressed process comprising one roughing and six cleaning procedures has been used for the processing of fluorite minerals. Subsequently, concentrates containing 93% fluorite, 2.5% calcite, and 3.5% sericite were obtained. Nonetheless, there is a lot of uncertainty regarding the current market and the cost of fluorite powders (93% ≤ CaF2 ≤ 97%). This is primarily because CaCO3 in the fluorite concentrates consumes sulfuric acid (H2SO4) and is also associated with the generation of heat energy and waste volume during the furnace reactions in the acidulation of fluorite concentrate. This creates a burden on anhydrous hydrofluoric acid (AHF) manufacturers because of the increased production costs. In such cases, leaching is the easiest solution. As shown in Figure 1, the fluorite concentrate is leached by waste hydrochloric acid (from a downstream chemical plant) after flotation.
Through this process, the calcite present in the fluorite concentrate was removed completely, but the CaF2 content increased to ~96% only and the remaining impurities could not be removed by this method. Moreover, sericite (SiO2) is a more important impurity than CaCO3 because it affects H2SO4 consumption during hydrofluoric acid (HF) or aluminum fluoride production. A number of side effects occur during the preparation owing to the hydrogen fluoride gas present in the reactor: 4HF (g) + SiO2 (s) = 2H2O (g) + SiF4 (g). Copious amounts of raw materials could be lost during production because of the high SiO2 content. Furthermore, against the background of this unprecedented situation caused by the pandemic, we need to find an effective method to desilicate fluorite concentrates before leaching.
Currently, during the direct flotation process, it is difficult to remove the silica completely via entrainment and the dissolved Ca ion might activate the sericite surface, as observed in our previous studies. In addition, further flotation cleaning was found to be ineffective. Therefore, we decided to use reverse flotation because it can be successful in cases where the gangue contains silicates (quartz or mica) and is floated with a collector of amine-type, while the valuable minerals are hydrophilic and are enriched in the underflow fraction [13,14,15]. This method was also reported to be the most widely used technology for the desilicification of various important minerals, i.e., iron ore and magnesite ore [16,17,18]. Several studies have been focusing on various amines and their derivatives that can be employed as cationic collectors in reverse flotation. Dodecylamine (DDA) is exceptionally effective as a collector of silicate minerals [19,20,21,22].
Conversely, fluorite depressants can efficiently enhance the flotation separation of sericite from fluorite. Liu and Zhang observed that citric acid (CA) might successfully eradicate Ca2+ ions from the chalcopyrite surface, thereby associated with the increase in the selective flotation separation between galena and chalcopyrite through the use of dextrin [23,24]. Additionally, Gao et al. and Gan et al. reported that CA exerts sufficient depressive effects on the oleate flotation of fluorite because of its robust chelating capacity with Mg2+ or Ca2+ [25,26]. Thus, these studies provided us with valuable insights into our analysis.
Consequently, it is worthwhile to develop a new method to achieve desilication and purification of fluorite concentrate before acid leaching. Although we have previously formulated an efficient two-stage depressing process for mineral processing, this study addresses the need for an efficient chemical scheme for improving the separation of sericite minerals in fluorite flotation. Fundamental analyses, such as micro-flotation, batch flotation, solution chemistry analysis, ZP measurements, and FTIR were conducted for the detailed information regarding the mechanism. This pilot study was carried out in the Xinyuan fluorite dressing plant and can potentially solve several long-standing complications regarding the shortage of high-quality fluorite concentrates.

2. Materials and Methods

We obtained pure fluorite and sericite samples from Hunan, China. The spectra of X-ray diffraction depicted in Figure 2 confirm the 98.41% and 91% purity of the fluorite and sericite samples, respectively. Grinding of the samples was performed using an agate mortar.
A micro-floatation test was conducted with the particle size of the fraction range from +37–74 μm. Further grinding of the samples was performed to obtain −5 μm size, and they were then used for ZP measurements and FTIR.
The fluorite concentrate in the real ore flotation test was a flotation separation concentrate supplied by Hunan Xinyuan Mineral Company. The samples consisted of 92.87% CaF2 and 2.82% SiO2.
The following suppliers were contacted for the chemically pure reagents: citric acid (H2C2O4) from Aladdin Biological Technology Ltd., Shanghai, China, and DDA (C12H27N) from Baisaiqin Chemical Technology Co., Ltd., Shanghai, China. Diluted solutions (0.1%) of HCl or NaOH were used for adjusting the pH.
Deionized water (DI, 18 mΩ·cm) was used for micro-flotation and test experiments.

2.1. Micro-Flotation Experiments

A hitch-groove flotation cell (40-mL), kept in a mechanically agitated flotation machine, was used to conduct the micro-flotation experiment. Particles (2.0 g) of the pure mineral were kept in a Plexiglas cell containing DI water (35 mL). For 2 min the pH of the resulting suspension was adjusted via the addition of NaOH or HCl, followed by depressant incorporation. Post 3 min conditioning of the suspension with the depressant, incorporation of the collector was made and provided 3 min agitation for the suspension.
For the flotation of the individual mineral, we collected and filtered the floated and unfloated particles and allowed them to dry. Individual micro-flotation tests were performed thrice and their average values were reported as the final result.

2.2. Measurement of Zeta Potential

Measurement for the ZP was carried out at 20 °C via the ZP analyzer (Zetasizer, Malvern, UK). The mineral suspensions with 40 mL of KCl (0.01 mol/L) and 0.016 g solids were prepared at a given collector concentration and pH and were used as the background electrolyte. The supernatant liquor obtained after a settling period of 5 min was used to measure the ZP measurement.

2.3. FTIR Spectral Analysis

We recorded the FTIR spectra of the samples on a Bruker Alpha FTIR spectrometer (Thermo, Waltham, MA, USA) at ~25 °C. Analysis of the samples was conducted by forming a KBr disc and scanned over a range of 400 to 4000 cm−1. Analysis procedures for the powder samples were as follows: the mineral powder (0.1 g) addition to the solution of the desired volume (25 mL) was carried out, followed by ultrasonication and stirring for 3 min each, and then treated for 6 min. After filtration, the solid material was obtained by using a vacuum drying method for the subsequent FTIR reflection spectroscopic measurements. The infrared spectrum of the untreated mineral was considered as the reference.

2.4. Batch Flotation Experiment

Fluorite concentrate ores were procured from Xinyuan Mining Co. Ltd. (Chenzhou, China) and were then divided into two portions. One portion was separated from the origin reagents using ultrasonic cleaning equipment, and the other was left unchanged. In an XFD-63 flotation cell (0.5 L) at a pH of approximately 6, the pulp was conditioned to solids (30%) with the depressant and collector. Fluorite concentrate (100 g) was used for flotation tests with l700 r/min flotation impeller speed. The tests of ore flotation were carried out according to the illustration described in Figure 3. Three replicates of the experiments were conducted and their mean values were regarded as the final results.

2.5. Pilot Test

The pilot test was performed in the Xinyuan factory, and the scale of the test was 25 t/day. The tests for the reverse flotation process and the direct leaching process were conducted with the selected collector and depressant. The results were then compared to obtain a detailed waste acid consumption analysis and the accurate removal rate of SiO2. Comparison diagram of pilot process is shown in Figure 4.

3. Results and Discussion

3.1. Micro-Flotation of Pure Minerals

Figure 5 depicts the flotation recoveries of sericite and fluorite as a function of pH of 1 × 10−4 mol/L DDA. Results show that sericite recovery is slightly elevated with the elevation in pH value. When DDA was used, the recovery of sericite was maintained above 60% in pH ranging from 2 to 3. Contrarily, the recovery of fluorite varied widely from 4.69 to 5.86% in a similar pH range, and a dramatic increase in fluorite recovery was observed at pH > 3. Therefore, a significant difference was observed between the recoveries of the two minerals in the strongly acidic pH range. At pH 2, 50.65% of sericite was recovered, which was sufficient for the flotation separation of sericite from fluorite, i.e., sericite could be selectively floated from fluorite with DDA as the collector at pH 2. For the following test, the pH was kept constant at pH 2.
Figure 6 demonstrates the sericite and fluorite recovery as a function of DDA dosage at pH 2 and the picture showing that the sericite recovery slowly increased with an elevation in the concentration of DDA. The selective flotation of sericite and fluorite can be achieved with a DDA concentration higher than 20 × 10−5 mol/L. Though, the sericite recovery was only ~69%. Moreover, owing to its hydrophilic property, hardly 31% of the sericite was removed from the pulp. Nevertheless, the recovery of fluorite increased rapidly when greater than 20 × 10−5 mol/L of concentration of DDA was there. This was because entrainment still exists because froth collapse from high concentration DDA is a long time. Although the result of the separation was satisfactory, it was difficult to operate the production process in a highly acidic environment (pH = 2) because of the potentially high cost and equipment corrosion. Thus, CA was used to depress fluorite, which hindered the adsorption with DDA. Figure 7 displays sericite and fluorite recovery as a function of CA dosage at pH 7.
Figure 7 reveals that the recovery of sericite was stable under weak acid or neutral conditions. Almost the same recovery was observed in the presence of CA as observed in its absence, indicating the weak depressive effect of CA on sericite flotation. Nevertheless, the recovery of fluorite sharply decreased when the CA concentration increased. When the CA dosage was 5 × 10−4 mol/L, the minimum fluorite recovery reached 4.83%. Based on these results, it was conjectured that CA could effectively depress fluorite at pH 7.
CA is a widely available trimacinic organic acid and could effectively adjust the value of pulp pH. The pH of the pulp was approximately 5, which was increased by the CA dosage (5 × 10−4 mol/L) as presented in Figure 7. In addition, the pH value of the solution was found to play the most imperative role in the flotation process (Figure 5). To determine the impact of depressing by CA in the flotation process, Figure 8 shows the recovery of sericite and fluorite with or without CA as a function of DDA dosage.
The obtained results in Figure 8 showed the satisfactory separation of sericite and fluorite by DDA in the presence of CA at a neutral pH, but high dosages of CA affected the pH, which can be elucidated with a comparison. In this test, the effect of DDA concentration was investigated in the absence and presence of CA at pH 5.
Furthermore, when the DDA concentration was 2 × 10−4 mol/L at pH 5, the floatability of the fluorite treated with CA was far lower than that of the untreated fluorite. The difference in floatability between the two conditions was approximately 55% when the DDA concentration was 3 × 10−4 mol/L. This result indicated that the fluorite surface pretreatment, which reduced the pH prior to DDA addition, was beneficial to the depressing behavior of fluorite. This finding could be ascribed to the decreasing of the pH level in the pulp because of the acidity of CA. However, the main reason is the decrease in the DDA amount adsorbed onto the fluorite surface treated with CA. It could be concluded that CA not only preserved the pH value of the pulp for the best flotation conditions for sericite but also effectively depressed the fluorite.

3.2. Zeta Potential (ZP)

To investigate the pH effect on the fluorite and sericite ZP in the presence of the collector, electrokinetic potentials were measured with CA (Figure 9). In the pH range of 2 to 11, the pure sericite minerals were always negatively charged, this is in a consistent with the results of the earlier study [27]. In the absence of reagents, fluorite had an isoelectric point (IEP) at pH 7.8, which was also in agreement with existing studies [28].
As seen in Figure 9a, when the pH was in the range 2–11, the ZP of sericite changed from negative to positive in the presence of DDA. This indicated that a high level of DDA amount has been absorbed on the sericite surface. Additionally, upon the addition of depressant CA, the ZP decreased by approximately 10 mV at the IEP ZP of sericite. This implied the slight absorption of CA on the negatively charged sericite surface and that the interaction between CA and the negatively charged sericite was weak. The depressant CA and the collector DDA incorporation increased the ZP of sericite by 35 mV, which suggested a strong electrostatic interaction of positively charged DDA with the negatively charged surface of sericite. The sericite ZP results in the presence of reagents also indicated that the quite stronger adsorption of DDA on the sericite surface than that of CA. Therefore, CA had little influence on the adsorption on the sericite surface. This is in good agreement with the results of the flotation depicted in Figure 6.
As shown in Figure 9b, a positively charged fluorite surface was observed at pH < 7.8 while it was negatively charged at pH > 7.8. After the addition of DDA to the pulp suspension, the ZP in the entire pH range increased, and rose more quickly at pH > 7.8, i.e., the ZP increased negatively, indicating that the interaction between DDA and fluorite surfaces gradually strengthened with increasing pH.
Additionally, depressant CA incorporation alters the fluorite ZP significantly, as it was decreased by an average of 25 mV during flotation, suggesting the strong depressant CA adsorption onto the fluorite surface. Unlike sericite, when both the collector DDA and the depressant CA were present, the fluorite ZP remained negative and only a slight increase than that in the presence of CA alone was observed in the pH range 2–11. This implied that the DDA adsorption on the surface of fluorite might be increasingly hindered by the presence of CA.

3.3. Solution Chemistry Analysis

The analysis of the solution chemistry of flotation is an effective way to examine the surface characteristics of the minerals and the reagents in the process of mineral flotation [29]. The solution chemistry equilibria of DDA are given as,
RNH 2 ( s ) = RNH 2 ( aq )   S = 10 4.70
RNH 3 + = RNH 2 ( aq ) + H +   K a = 10 10.63
2 RNH 3 + = ( RNH 3 2 + ) 2 2 +   K d = 10 2.08
RNH 3 + + RNH 2 ( aq ) = [ RNH 3 + · RNH 2 ( aq ) ]   K im = 10 3.12
The solution chemistry equilibria of CA are as follows:
H 3 Cit = H 2 Cit   + H +   K a 1 = 10 3.13
H 2 Cit   = HCit   2 + H +   K a 2 = 10 4.76
HCit   2 = Cit   3 + H +   K a 3 = 10 6.4
Cit   3 = Cit   4 + H +   K a 4 = 10 11.6
Based on the above formulas, at DDA concentration (CDDA) = 2 × 10−4 mol/L, Figure 10 and Figure 11 demonstrate the component distributions of DDA and CA, respectively, as a function of pH.
Figure 10 indicated the precipitation of neutral RNH2 molecule at pH 10.04, and its ionic forms (RNH3)22+ and RNH3+ dominated in a pH range of 2.0–9.5. The maximum ion–molecular complex was observed at pH 9.85. Moreover, the sericite surface was always negative because the pH was less than 10. The primary species of the collector are RNH2·RNH3+, RNH3+, and (RNH3)22+, so the electrostatic adsorption was strong between the two. Nevertheless, at pH 7.8–10, the fluorite surface changed from positive to negative, i.e., the DDA adsorption capacity on the fluorite surface increased in a weak alkaline environment, which is in agreement with the flotation data that was obtained earlier.
As seen in Figure 11, the Cit3− species reached a maximum at pH 9.9, showing consistency with the flotation behavior of fluorite. In a strongly alkaline medium, the main CA species was Cit3− and they played a significant role in the inhibition of fluorite. Certain studies have shown that the reactions of Ca2+ and Cit3− ions were thermodynamically favored at pH in the range 5.5–13.0 [31]. Thus, anionic Cit3− was adsorbed onto the negatively charged fluorite surface at pH > IEP 7.8 via chemical adsorption process rather than electrostatic attraction. In addition, fluorite ZP showed a significant difference when treated with both CA and DDA. Compared to the ZP in the presence of CA alone, the ZP of fluorite in the presence of both CA and DDA shifted to a slightly more acidic value. We assumed that DDA was physically adsorbed onto the fluorite surface in a similar manner to the sericite surface. However, in a pH range from 2–11, the pH of the fluorite surface treated by both CA and DDA changed to high alkaline values. Thus, the assumption was invalid. Furthermore, this result implied that Cit ions in the pulp suspension transferred to the fluorite surfaces as the hydrolysis progressed and that additional chelates could be formed.

3.4. FTIR Results

The above experiments and analyses demonstrated that the depressant CA and the collector DDA could be selectively adsorbed onto sericite and fluorite surfaces, but the adsorption mechanism remains unclear and needs to be elucidated. Here, we analyze the FTIR spectra of sericite and fluorite to study the possible adsorption mechanism.
Sericite has two clear characteristic peaks at 3628 and 1024 cm−1 (Figure 12a), which were associated with stretching vibration of the Al–OH groups and the in-plane stretching of the Si-O-Si (Al) or Si (Al)-O groups, respectively [32]. The peaks at 2357 and 2360 cm−1 were ascribed to the CO2 impurities (exclusion). For the DDA spectrum, two peaks at 2918 and 2844 cm−1 were attributed to –CH stretching. Similarly, the peak appearing at 2364 cm−1 and having a shoulder at 2335 cm−1 was attributed to the stretching of –CN group [33,34]. The spectra obtained for sericite with DDA indicated that the –CH3 or –CH2 stretching bands appeared at 2847 and 2919 cm−1. Additional band shifts of DDA could not be used to determine the electrostatic adsorption of DDA onto the surface of sericite. Furthermore, compared to the FTIR spectrum of the sericite treated with DDA only, the sericite treated with both CA and DDA did not show any CA characteristic peak, which confirmed the absence of CA absorption onto the sericite surface.
For the fluorite system, as shown in Figure 12b, similar peaks (2933 and 2849 cm−1) appeared for the fluorite surface with DDA. This suggested the occurrence of an electrostatic adsorption process similar to that of sericite with DDA, and this in turn indicated that the selectivity of DDA was poor. In the FTIR spectrum of CA, the peaks observed at 1715, 3370, 1417, and 799 cm−1 were due to the presence of –COOH groups, –OH groups, C–O groups, and C–H stretching, respectively. In comparison with the FTIR spectrum of the purified fluorite, the fluorite exposed to DDA and CA showed characteristic absorption peaks at 1715 and 3370 cm−1 owing to the presence of –COOH groups and weakened vibrations of –OH groups, respectively. Moreover, the peak at 1393 cm−1, caused by C–O groups, represented a band shift of 24 cm−1 and demonstrated the chemisorption of CA on the fluorite surface. In the spectrum, fluorite treated with CA and DDA showed the change in characteristic absorption peaks as well as presented the symmetrical stretching vibration of chelates in the range 1500–1700 cm−1. Because of the disappearance of the stretching vibration of –CH groups (2933 and 2849 cm−1), we deduced that the DDA adsorption was hindered by the CA chemisorbed onto the fluorite surface.

3.5. Batch Flotation Experiment Results

Based on the optimized micro-flotation test conditions, two tests were conducted on a fluorite concentrate containing 92.87% CaF2 (fluorite), 2.82% SiO2 (sericite including 1.17% Al2O3), and 3.14% CaCO3 (calcite), which was procured from the Xinyuan mine (Hunan, China). Most of the fluorite and sericite minerals in the fluorite powder were distributed in the +10–37μm range. Fewer amounts as sericite were set in a fluorite combination (10μm). The images of the feed powders obtained via an optical microscope are shown in Figure 13.
As depicted in Figure 13, the average size of fluorite was clearly less than that of sericite. Additionally, at 10μm, the sericite was present with the fluorite. Thus, it is difficult to further enrich the fluorite concentrate because the fine particles of sericite could be easily entrained [35] and Ca2+ ions could be activated by NaOl [27]. The detailed flowsheet and reagent scheme of the closed-circuit flotation are shown in Figure 3. The conditions for the comparison tests of flotation and the obtained results are represented in Table 1 and Figure 14, respectively.
Figure 14 displays the results of the comparison tests of direct flotation and reverse flotation. Simple 1 was the fluorite concentrate and was retrieved from the flotation plant site. The unwashed simple 2 was treated with sodium silicate (SS). The CaF2 content of the concentrate increased slightly, but the SiO2 content showed no such changes. The CaCO3 content of the concentrate decreased when the fluorite concentrate was washed (simple 3), largely due to the inhibition of the impurity minerals caused by washing. However, the SiO2 and Al2O3 contents were unaffected. This proved that sericite could not be removed easily by direct flotation. When the CA and DDA dosages were 5.0 kg/t and 50 g/t, respectively, fluorite content increased to 95.07%, whereas SiO2 and Al2O3 content decreased from 2.82 to 1.28% and from 1.17 to 0.74%, respectively. For comparison, to acquire the flotation performance via CA + DDA for cleaned samples, it was found that the residual reagent (NaOl) used in the production and for the activation of sericite affected the collection of DDA. When simple 5 was cleaned, the CaF2 content of the concentrate increased to 95.89% and SiO2 recovery was only 30.49%. Both SiO2 and Al2O3 content dropped. The root cause of this phenomenon was the ratio of SiO2 to Al2O3 in sericite (2:1). Furthermore, the removal rate of sericite was 69.51%. Therefore, the reverse flotation of CA + DDA showed great potential for industrial applications. Owing to the volatility of the samples in batch flotation experiments, the grade and recovery of fluorite products were verified by subsequent semi-industrial tests.

3.6. Pilot Test Results

The process of the pilot test is illustrated in Figure 4. The primary purpose of the pilot test was to verify the feasibility of the batch flotation experiments. The results of the comparison tests for the direct leaching (process 1 plan date: May 10–17) and the reverse flotation + leaching (process 2 plan date: May 15–21) processes are depicted in Figure 15, Figure 16, and Figure 17. Figure 15 presents a comparison of the grade of fluorite concentrates obtained in processes 1 and 2. The grade of fluorite in process 2 was ~1.5% higher than that obtained in process 1. According to the current market conditions, the price of fluorite powder (CaF2 ≥ 97%) per ton is USD 39.67 higher than the original price of fluorite powder (95% ≤ CaF2 < 97%). Moreover, the SiO2 content of the concentrate in process 2 was ~1.0% lower than that in process 1 (Figure 16). This result also contributed to the reduction in the consumption of sulfuric acid in the downstream hydrofluoric acid process and reduced the impurities in the product. In addition, the recovery of fluorite concentrate was lowered from 76.84 to 73.59% only, so the loss of fluorite is extremely small. Although the results of the pilot test have certain limitations, the new reverse flotation + leaching technology can dramatically reduce the potential costs and environmental impact. The new process not only contributed to the safety of AHF production plants but also reported a huge increase in the forecasted profits (~USD 1,4374.06 per day) (Table 2). Naturally, the economic benefits would also significantly improve with the increased price of high-grade fluorite powder (CaF2 ≥ 97%).

4. Conclusions

This study found that reverse flotation was an efficient approach for the desilication of fluorite concentrates. Through micro-flotation tests, it was confirmed that the fluorite and sericite separation under acidic conditions or with CA + DDA could be quite successful. Additionally, a dominant electrostatic attraction force was detected in the interaction of DDA with sericite and fluorite, and the mechanism of CA was confirmed by ZP measurements, solution chemistry analysis, and FTIR. Furthermore, we found that the content of SiO2 and Al2O3 decreased during the batch flotation experiment. The results of the pilot test proved that the new reverse flotation + leaching technology could dramatically reduce the potential environmental impact and costs, thereby significantly improving the economic benefits by satisfying the current demands of the market.

Author Contributions

Formal analysis, C.Z.; investigation, J.G. and F.L.; methodology, Y.H.; resources, W.S. and Z.L.; writing—original draft, C.Z.; writing—review and editing, J.G. and C.Z.; project administration, W.S and Y.H. All authors have read and agreed to the published version of the manuscript.

Funding

This research was funded by the National Natural Science Foundation of Guizhou Province (qian ke he ji chu [2020]1Y218); the Young Talents Foundation of Education Department of Guizhou Province (qian jiao he KY zi [2019]136) and the Scientific and Technological Innovation Platform of Liupanshui (52020-2019-05-04 and 52020-2019-05-06); the Academician Workstation of Liupanshui Normal University (qiankehepingtairencai [2019]5604hao); the Fund of Liupanshui Normal University (LPSSYKJTD201906).

Data Availability Statement

Not applicable.

Conflicts of Interest

The authors declare no conflict of interest.

References

  1. Zhang, Y.; Song, S. Beneficiation of fluorite by flotation in a new chemical scheme. Miner. Eng. 2003, 16, 597–600. [Google Scholar] [CrossRef]
  2. Gao, Z.; Wang, C.; Sun, W.; Gao, Y.; Kowalczuk, P.B. Froth flotation of fluorite: A review. Adv. Colloid Interface Sci. 2021, 290, 102382. [Google Scholar] [CrossRef]
  3. Shuai, F.; Xu, L.; Wu, H.; Jia, T.; Lu, Z.; Wei, S.; Hu, Y. Adsorption of Pb(II)/benzohydroxamic acid collector complexes for ilmenite flotation. Miner. Eng. 2018, 126, 16–23. [Google Scholar] [CrossRef]
  4. Gao, Y.; Gao, Z.; Sun, W.; Hu, Y. Selective flotation of scheelite from calcite: A novel reagent scheme. Int. J. Miner. Process. 2016, 154, 10–15. [Google Scholar] [CrossRef]
  5. Kou, J.; Tao, D.; Xu, G. Fatty acid collectors for phosphate flotation and their adsorption behavior using QCM-D. Int. J. Miner. Process. 2010, 95, 1–9. [Google Scholar] [CrossRef]
  6. Hu, Y.-H.; Yang, F.; Sun, W. The flotation separation of scheelite from calcite using a quaternary ammonium salt as collector. Miner. Eng. 2011, 24, 82–84. [Google Scholar] [CrossRef]
  7. Liu, C.; Zhou, M.; Xia, L.; Fu, W.; Zhou, W.; Yang, S. The utilization of citric acid as a depressant for the flotation separation of barite from fluorite. Miner. Eng. 2020, 156, 106491. [Google Scholar] [CrossRef]
  8. Filippov, L.; Filippova, I.; Severov, V. The use of collectors mixture in the reverse cationic flotation of magnetite ore: The role of Fe-bearing silicates. Miner. Eng. 2010, 23, 91–98. [Google Scholar] [CrossRef]
  9. Ma, X.; Marques, M.; Gontijo, C. Comparative studies of reverse cationic/anionic flotation of Vale iron ore. Int. J. Miner. Process. 2011, 100, 179–183. [Google Scholar] [CrossRef]
  10. Santos, E.P.; Dutra, A.J.; Oliveira, J.F. The effect of jojoba oil on the surface properties of calcite and apatite aiming at their selective flotation. Int. J. Miner. Process. 2015, 143, 34–38. [Google Scholar] [CrossRef]
  11. Liu, H.; Khoso, S.A.; Sun, W.; Zhu, Y.; Han, H.; Hu, Y.; Kang, J.; Meng, X.; Zhang, Q. A novel method for desulfurization and purification of fluorite concentrate using acid leaching and reverse flotation of sulfide. J. Clean. Prod. 2019, 209, 1006–1015. [Google Scholar] [CrossRef]
  12. Zhang, C.; Sun, W.; Hu, Y.; Tang, H.; Yin, Z.; Guan, Q.; Gao, J. Investigation of two-stage depressing by using hydrophilic polymer to improve the process of fluorite flotation. J. Clean. Prod. 2018, 193, 228–235. [Google Scholar] [CrossRef]
  13. Mowla, D.; Karimi, G.; Ostadnezhad, K. Removal of hematite from silica sand ore by reverse flotation technique. Sep. Purif. Technol. 2008, 58, 419–423. [Google Scholar] [CrossRef]
  14. Mohammadkhani, M.; Noaparast, M.; Shafaei, S.; Amini, A.; Amini, E.; Abdollahi, H. Double reverse flotation of a very low grade sedimentary phosphate rock, rich in carbonate and silicate. Int. J. Miner. Process. 2011, 100, 157–165. [Google Scholar] [CrossRef]
  15. Yang, S.; Xu, Y.; Liu, C.; Huang, L.; Huang, Z.; Li, H. The anionic flotation of fluorite from barite using gelatinized starch as the depressant. Colloids Surfaces A Physicochem. Eng. Asp. 2020, 597, 124794. [Google Scholar] [CrossRef]
  16. Lin, L.; Jiong-tian, L.; Yong-tian, W.; Yi-jun, C.; Hai-jun, Z.; He-sheng, Y. Experimental research on anionic reverse flotation of hematite with a flotation column. Procedia Earth Planet. Sci. 2009, 1, 791–798. [Google Scholar] [CrossRef] [Green Version]
  17. Abaka-Wood, G.B.; Addai-Mensah, J.; Skinner, W. A study of flotation characteristics of monazite, hematite, and quartz using anionic collectors. Int. J. Miner. Process. 2017, 158, 55–62. [Google Scholar] [CrossRef]
  18. Liu, G.; Zhong, H.; Hu, Y.; Zhao, S.; Xia, L. The role of cationic polyacrylamide in the reverse flotation of diasporic bauxite. Miner. Eng. 2007, 20, 1191–1199. [Google Scholar] [CrossRef]
  19. Xu, L.; Longhua, X.; Tian, J.; Wu, H.; Wang, L.; Yang, Y.; Wang, Z. Synergistic effect of mixed cationic/anionic collectors on flotation and adsorption of muscovite. Colloids Surfaces A Physicochem. Eng. Asp. 2016, 492, 181–189. [Google Scholar] [CrossRef]
  20. Wang, L.; Hu, Y.; Liu, J.; Sun, Y.; Sun, W. Flotation and adsorption of muscovite using mixed cationic–nonionic surfactants as collector. Powder Technol. 2015, 276, 26–33. [Google Scholar] [CrossRef]
  21. Sahoo, H.; Rath, S.S.; Das, B.; Mishra, B.K. Flotation of quartz using ionic liquid collectors with different functional groups and varying chain lengths. Miner. Eng. 2016, 95, 107–112. [Google Scholar] [CrossRef]
  22. Lima, N.P.; Valadão, G.E.; Peres, A.E. Effect of amine and starch dosages on the reverse cationic flotation of an iron ore. Miner. Eng. 2013, 45, 180–184. [Google Scholar] [CrossRef]
  23. Liu, Q.; Zhang, Y. Effect of calcium ions and citric acid on the flotation separation of chalcopyrite from galena using dextrin. Miner. Eng. 2000, 13, 1405–1416. [Google Scholar] [CrossRef]
  24. Liu, C.; Zheng, Y.; Yang, S.; Fu, W.; Chen, X. Exploration of a novel depressant polyepoxysuccinic acid for the flotation sep-aration of pentlandite from lizardite slimes. Appl. Clay Sci. 2020, 105939. [Google Scholar] [CrossRef]
  25. Gan, W.; Crozier, B.; Liu, Q. Effect of citric acid on inhibiting hexadecane–quartz coagulation in aqueous solutions containing Ca2+, Mg2+ and Fe3+ ions. Int. J. Miner. Process. 2009, 92, 84–91. [Google Scholar] [CrossRef]
  26. Gao, Z.; Gao, Y.; Zhu, Y.; Hu, Y.; Sun, W. Selective Flotation of Calcite from Fluorite: A Novel Reagent Schedule. Minerals 2016, 6, 114. [Google Scholar] [CrossRef] [Green Version]
  27. Hu, Y.; He, J.; Zhang, C.; Zhang, C.; Sun, W.; Zhao, D.; Chen, P.; Han, H.; Gao, Z.; Liu, R.; et al. Insights into the activation mechanism of calcium ions on the sericite surface: A combined experimental and computational study. Appl. Surf. Sci. 2018, 427, 162–168. [Google Scholar] [CrossRef]
  28. Gao, Z.; Sun, W.; Hu, Y.-H.; Liu, X.-W. Anisotropic surface broken bond properties and wettability of calcite and fluorite crystals. Trans. Nonferrous Met. Soc. China 2012, 22, 1203–1208. [Google Scholar] [CrossRef]
  29. Somasundaran, P.; Wang, D. Solution Chemistry: Minerals and Reagents; Elsevier: Amsterdam, The Netherlands, 2006; ISBN 0080465072. [Google Scholar]
  30. Al-Khaldi, M.; Nasr-El-Din, H.; Mehta, S.; Al-Aamri, A. Reaction of citric acid with calcite. Chem. Eng. Sci. 2007, 62, 5880–5896. [Google Scholar] [CrossRef] [Green Version]
  31. Nagy, N.M.; Konya, J.; Kónya, I. Ion-exchange processes of lead and cobalt ions on the surface of calcium-montmorillonite in the presence of complex-forming agents II. The effect of DTPA, tartaric acid and citric acid on the sorption of lead ions on calcium-montmorillonite. Colloids Surfaces A Physicochem. Eng. Asp. 1998, 137, 243–252. [Google Scholar] [CrossRef]
  32. Tian, J.; Gao, H.; Guan, J.; Ren, Z. Modified floc-flotation in fine sericite flotation using polymethylhydrosiloxane. Sep. Purif. Technol. 2017, 174, 439–444. [Google Scholar] [CrossRef]
  33. Carrara, C.; Irusta, S.; Lombardo, E.; Cornaglia, L. Study of the Co-VPO interaction in promoted n-butane oxidation catalysts. Appl. Catal. A Gen. 2001, 217, 275–286. [Google Scholar] [CrossRef]
  34. Gupta, N.; Balomajumder, C.; Agarwal, V.K. Adsorption of cyanide ion on pressmud surface: A modeling approach. Chem. Eng. J. 2012, 191, 548–556. [Google Scholar] [CrossRef]
  35. Warren, L.J. Determination of the contributions of true flotation and entrainment in batch flotation tests. Int. J. Miner. Process. 1985, 14, 33–44. [Google Scholar] [CrossRef]
Figure 1. Acid leaching process of fluorite minerals in the Xinyuan dressing plant.
Figure 1. Acid leaching process of fluorite minerals in the Xinyuan dressing plant.
Minerals 11 00555 g001
Figure 2. Spectra of X-ray diffraction for (a) fluorite and (b) sericite samples used for the flotation tests.
Figure 2. Spectra of X-ray diffraction for (a) fluorite and (b) sericite samples used for the flotation tests.
Minerals 11 00555 g002
Figure 3. Flowsheet of the flotation tests.
Figure 3. Flowsheet of the flotation tests.
Minerals 11 00555 g003
Figure 4. Comparison flowsheet of the pilot test (1. Direct leaching; 2. Reverse flotation before leaching).
Figure 4. Comparison flowsheet of the pilot test (1. Direct leaching; 2. Reverse flotation before leaching).
Minerals 11 00555 g004
Figure 5. Depicted the recovery of sericite and fluorite as a function of pH via DDA as a collector (concentration = 1 × 10−4 mol/L).
Figure 5. Depicted the recovery of sericite and fluorite as a function of pH via DDA as a collector (concentration = 1 × 10−4 mol/L).
Minerals 11 00555 g005
Figure 6. Recovery of sericite and fluorite as a function of DDA dosage at pH 2.
Figure 6. Recovery of sericite and fluorite as a function of DDA dosage at pH 2.
Minerals 11 00555 g006
Figure 7. Recovery of sericite and fluorite as a function of CA dosage at pH 7.
Figure 7. Recovery of sericite and fluorite as a function of CA dosage at pH 7.
Minerals 11 00555 g007
Figure 8. Recovery of sericite and fluorite both in the presence and absence of CA as a function of DDA dosage.
Figure 8. Recovery of sericite and fluorite both in the presence and absence of CA as a function of DDA dosage.
Minerals 11 00555 g008
Figure 9. ZP of (a) sericite and (b) fluorite as a function of pH in various conditions.
Figure 9. ZP of (a) sericite and (b) fluorite as a function of pH in various conditions.
Minerals 11 00555 g009
Figure 10. Species distribution diagram of DDA as a function of pH. (DDA total conc. = 2.0 × 10−4 mol/L.)
Figure 10. Species distribution diagram of DDA as a function of pH. (DDA total conc. = 2.0 × 10−4 mol/L.)
Minerals 11 00555 g010
Figure 11. Species distribution diagram of CA as a function of pH (25 °C and 1 atm) [30].
Figure 11. Species distribution diagram of CA as a function of pH (25 °C and 1 atm) [30].
Minerals 11 00555 g011
Figure 12. (a) Fourier transform infrared spectra of sericite pre- and post-binding with DDA and CA. (b) Fourier transform infrared spectra of fluorite pre- and post-binding with DDA and CA.
Figure 12. (a) Fourier transform infrared spectra of sericite pre- and post-binding with DDA and CA. (b) Fourier transform infrared spectra of fluorite pre- and post-binding with DDA and CA.
Minerals 11 00555 g012
Figure 13. Images of feed material by microscope (F1—fluorite; Q—sericite).
Figure 13. Images of feed material by microscope (F1—fluorite; Q—sericite).
Minerals 11 00555 g013
Figure 14. Results of the comparison tests of flotation (direct and reverse).
Figure 14. Results of the comparison tests of flotation (direct and reverse).
Minerals 11 00555 g014
Figure 15. Comparison of the grade of fluorite concentrates in processes 1 and 2.
Figure 15. Comparison of the grade of fluorite concentrates in processes 1 and 2.
Minerals 11 00555 g015
Figure 16. Comparison of the SiO2 content of the concentrates in processes 1 and 2.
Figure 16. Comparison of the SiO2 content of the concentrates in processes 1 and 2.
Minerals 11 00555 g016
Figure 17. Results of mineral recovery from the fluorite concentrate in processes 1 and 2.
Figure 17. Results of mineral recovery from the fluorite concentrate in processes 1 and 2.
Minerals 11 00555 g017
Table 1. The conditions for the comparison tests of flotation.
Table 1. The conditions for the comparison tests of flotation.
SampleCondition
1Fluorite concentrate
2Direct flotation (unwashed ore) + SS (200 g/t) + NaOl (50 g/t)
3Direct flotation (washed ore) + SS (200 g/t) + NaOl (50 g/t)
4Reverse flotation (unwashed ore) + CA (5 kg/t) + DDA (50 g/t)
5Reverse flotation (washed ore) + CA (5 kg/t) + DDA (50 g/t)
Table 2. Forecast profits based on pilot test results (2000 t/d).
Table 2. Forecast profits based on pilot test results (2000 t/d).
ConsumptionUnit Price (USD/t)1# (t/d)2# (t/d)∆ Profit (USD/d)
Fluorite powder (95 ≤ CaF2 < 97%)154.04614.72/+17,583.32
Fluorite powder (CaF2 ≥ 97%)190.71/588.72
Diluted hydrochloric58.6873.7749.18+1442.94
Citric acid440.1/10−4401
Dodecylamine3374.1/0.1−337.41
Waste water treatment cost2.9341803.591727.30+76.29
Power0.3814234.45224.53+9.92
Total///+14,374.06
Publisher’s Note: MDPI stays neutral with regard to jurisdictional claims in published maps and institutional affiliations.

Share and Cite

MDPI and ACS Style

Zhang, C.; Gao, J.; Hu, Y.; Sun, W.; Lv, F.; Liu, Z. Clean and Feasible Utilization of High Silica Fluorspar Powder via Reverse Flotation: A Pilot Study. Minerals 2021, 11, 555. https://doi.org/10.3390/min11060555

AMA Style

Zhang C, Gao J, Hu Y, Sun W, Lv F, Liu Z. Clean and Feasible Utilization of High Silica Fluorspar Powder via Reverse Flotation: A Pilot Study. Minerals. 2021; 11(6):555. https://doi.org/10.3390/min11060555

Chicago/Turabian Style

Zhang, Chenhu, Jiande Gao, Yuehua Hu, Wei Sun, Fei Lv, and Zhenjun Liu. 2021. "Clean and Feasible Utilization of High Silica Fluorspar Powder via Reverse Flotation: A Pilot Study" Minerals 11, no. 6: 555. https://doi.org/10.3390/min11060555

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.

Article Metrics

Back to TopTop