Article

Thermal and Calorimetric Investigations of Some Phosphorus-Modified Chain Growth Polymers 2: Polystyrene

by
Malavika Arun
1,*,
Stephen Bigger
1,
Maurice Guerrieri
1,
Paul Joseph
1,* and
Svetlana Tretsiakova-McNally
2
1
Institute of Sustainable Industries and Liveable Cities, Victoria University, P.O. Box 14428, Melbourne, VIC 8001, Australia
2
Belfast School of Architecture and the Built Environment, Ulster University, Newtownabbey BT37 0QB, UK
*
Authors to whom correspondence should be addressed.
Polymers 2022, 14(8), 1520; https://doi.org/10.3390/polym14081520
Submission received: 22 February 2022 / Revised: 29 March 2022 / Accepted: 6 April 2022 / Published: 8 April 2022
(This article belongs to the Section Polymer Composites and Nanocomposites)

Abstract

:
In this paper, we report on the thermal degradation behaviours and combustion attributes of some polymers based on polystyrene (PSt). Here, both additive and reactive strategies were employed, through the bulk polymerization route, where the modifying groups incorporated P-atom in various chemical environments. These included oxidation states of III or V, and the loading of phosphorus was kept at ca. 2 wt.% in all cases. The characterization techniques that were employed for the recovered products included spectroscopic, thermal, and calorimetric. It was found that the presence of different modifying groups influenced the degradation characteristics of the base polymer, and also exerted varying degrees of combustion inhibition. In all cases, the modification of the base matrix resulted in a noticeable degree of fire retardance as compared to that of the virgin material. Therefore, some of the modifications presented have the potential to be explored on a commercial scale.

1. Introduction

Polystyrene (PSt) is a relatively inexpensive, readily available, and transparent thermoplastic polymer that is used for a wide number of applications [1]. The monomer, styrene, may also be copolymerised with other monomers to produce co- and/or ter-polymers, often having improved properties [2]. Some of the modified systems can be utilized for specific functions, such as removing heavy metals from water [3,4,5,6]. Some of the multicomponent systems include styrene acrylonitrile (SAN), acrylonitrile-butadiene-styrene (ABS) polymers, styrene-butadiene rubber (SBR), etc. Furthermore, there are two types of polystyrene foams that are commercially available: expanded polystyrene (EPS) and extruded polystyrene (XPS). Expanded polystyrene is generally used for food packaging applications and XPS, which is a higher density foam, is used in the building sector [7]. One of the disadvantages of PSt, despite its useful characteristics, is its relatively high flammability. When ignited, polystyrene and its copolymers often burn quickly with a visible flame, releasing volatiles including styrene monomer, oligomers, lower hydrocarbons such as benzene, lower alkylbenzenes [8], etc. During the burning process, polystyrene can also melt, flow, and drip, which can lead to an increased fuel load feeding into enhanced flame spread [9]. Generally, combustion of unmodified polystyrene produces a minimal amount of char residue.
Polystyrene homopolymer generally starts degrading at a temperature around 270 °C and continues until 425 °C under normal conditions in air. Through random main-chain cleavages and associated processes, PSt forms varying amounts of a number of compounds. These include styrene, benzaldehyde, styrene oxide, acetophenone, and l-phenylethanol. Such scissions generally originate from structural irregularities, such as head-to-head linkages and other minor structures, and are predominant at relatively lower temperatures [10]. Styrene and benzaldehyde are found to be the prominent fractions among the decomposition products [11]. Like the majority of main-chain carbon polymers, it has long been established that the thermal decomposition of polystyrene generally occurs in three steps: initiation, propagation, and termination, which follows a radical chain mechanism [12]. Most of the low molecular weight fragments that are produced upon the thermal or thermo-oxidative degradation of styrenic polymers can form combustible mixtures with ambient air. These mixtures, in the presence of a suitable ignition source, can subsequently undergo flaming combustion.
With a view to address the flammability issue of polystyrene-based materials, several flame retarding strategies have been developed. In this context, for adequately fireproofing the finished products, both the additive and reactive approaches are often adopted [13,14,15,16,17,18,19]. Given the environmental implications and the need to use relatively higher loadings, the use of halogen-based fire retardants (FRs) and heavy metal-based compounds or their combinations are progressively being discouraged. In this context, FRs based on phosphorus have gained prominence, especially in recent years [20,21,22]. For achieving an acceptable level of fire retardance, formulation based on bio-sourced FRs are also used [23,24,25]. The relative predominance of condensed- and vapour-phase activities of phosphorus-based FRs depend both on the nature of the P-containing additive or reactive (i.e., chemical class of the compound and the oxidation state of the P-atom), as well as on the chemical constitution of parent polymeric matrix [26,27,28,29,30,31].
Both additive and reactive strategies have been employed to bring about noticeable improvements in the flame retardance of polystyrene at a relatively low loading of phosphorus (ca. 2.0 wt.% in all cases). Here, additives were simply incorporated into the monomer or initiator mixture to form physical mixtures, whereas the polymerizable compounds were added into the main monomer mixture during the syntheses of copolymers. All polymerization reactions were conducted through the bulk route, with minor adaptations if necessary, as previously reported [32,33]. The novelty of the present work stems from the utilization of a number of phosphorus-bearing compounds or groups, where the P-atom exhibited its valence states of III or V, and that the chemical environments of these groups also belonged to different categories (i.e., phosphites, phosphates, phosphonates, phosphorylaminoester, phosphine, and phosphine oxide). The central idea here was to gauge the influences, through a systematic approach, of the oxidation states and chemical environments of the modifying groups on the combustion properties of polystyrene. Hence, the loading of P (i.e., ca. 2 wt.%) was kept constant in all cases.

2. Materials and Methods

2.1. Materials

Except for the additives 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide (DOPO) and diethyl-1-propylphosphonate (Thermofisher Scientific, Melbourne, Australia), all other chemicals and solvents were purchased from the Aldrich Chemical Company, Melbourne, Australia. The solid compounds were used as received, whereas liquid reagents and solvents were optionally dried by keeping them over molecular sieves (4 Å). The thermally labile initiators and monomers were stored under sub-ambient temperatures in a refrigerator, or in a freezer, as required. A proprietary inhibitor column was employed to remove the inhibitor, tert-butylcatechol, from the styrene monomer prior to use. The necessary precursors, comonomers, and the additive, diethylbenzylphosphonate (DEBP), were synthesized by following procedures as given in Part I (i.e., pertaining to polymethyl methacrylate) of our previous work [34]. The other additives and monomers studied included triphenylphosphine (TPP), triphenylphosphineoxide (TPPO), diethylphosphite (DEHPi), triethylphosphite (TEPi), triethylphosphate (TEPa), diethylpropylphosphonate (DEPP), diethyl-1-(acryloyloxyethyl)phosphonate (DE-1-AEP), acrylicacid-2-[(diethoxyphosphoryl)methylamino] ester (ADEPMAE), diethyl-2-(acryloyloxy)ethylphosphate (DEAEPa), and diethyl-p-vinylbenzylphosphonate (DEpVBP). The chemical structures of both the additives and reactives are also given in our previous work [34].

2.2. A Typical Procedure for Bulk Polymerization

The procedure was based on a previously published work where minor adjustments to the curing regime were affected [33]. Here, the required amount of monomer(s) and initiators were stirred thoroughly in a conical flask under a nitrogen atmosphere for ca. 5 h at 70 °C, until a visible increase in the viscosity was observed. The calculated amount of the additive or reactive was then added and stirred for another 1 h. The resultant mixture was subsequently poured into an aluminium pan of ca. 50 mL volume and the pan was stoppered with an aluminium lid. The pan was placed in an air oven preheated to 40 °C and kept for curing for about 20 h. In the second stage of curing, the temperature of the oven was raised to 60 °C for 8 h. After another 20 h of curing at 80 °C, the contents of the pan were allowed to cure again for a period of 3 h at 100 °C before being cooled to room temperature. The final plaque was then extracted from the aluminium pan. Again, a fixed phosphorus loading of 2 wt.% was used. The structures of the additives and comonomers used in the present study are given previously [34]. The required amounts of the modifying compounds relative to the monomer and associated details are given in Table 1.

2.3. Characterization

The structures and purities of the additives, precursors, monomers and polymeric materials were established primarily through NMR spectroscopy. For this, a Bruker 600 MHz instrument was employed, and the spectra were run in deuterated solvents (CDCl3, or d6-DMSO) at ambient probe conditions. The signals were calibrated against residual proton signal of the solvent, or phosphoric acid as the external calibrant, as required. The raw data were processed by using proprietary software from the manufacturer (TopSpin 4.0.8).
Thermo-gravimetric (TGA) analyses on the polymeric products were run in nitrogen at 10 °C min−1 and 60 °C min−1, from 30 to 900 °C, using a Mettler-Toledo instrument. The set heating rate of 60 °C min−1 was chosen with a view to compare and correlate the results from the TGA experiments to those of other calorimetric techniques, such as the pyrolysis combustion flow calorimetry (PCFC) technique. Differential scanning calorimetry (DSC) runs were primarily used to estimate the heats of pyrolysis of the various polymeric materials. For this purpose, the thermograms were recorded in a nitrogen atmosphere at a heating rate of 10 °C min−1, from 30 to 550 °C, using a Mettler-Toledo instrument. The glass transition temperatures of the samples were also obtained from the DSC curves.
The combustion behaviours of the various polymeric products were measured through pyrolysis combustion flow calorimetry (PCFC) technique, also known as ‘micro combustion calorimetry’ (MCC). This is a small-scale calorimetric testing method increasingly being used to analyse the fire behaviour of various solid materials when subjected to a forced non-flaming combustion, under anaerobic or aerobic conditions. The details of this technique, including working principle and information regarding the parametric outputs, are published elsewhere [35,36,37,38]. In the present work, PCFC runs were carried out using a FAA Micro Calorimeter at 1 °C min−1. The samples were pyrolyzed in an inert atmosphere with nitrogen at a temperature range of 100–750 °C and averages over triplicate runs are reported. The heats of combustion of various polymeric materials were deduced by performing a ‘complete’ combustion in pure oxygen, using an IKA C200 ‘Bomb’ calorimeter (IKA, Oxford, UK). Pelleted samples, weighing ca. 0.5 g, were placed inside a ‘bomb’ cell. The instrument was previously calibrated using recrystallized benzoic acid and, for each sample, triplicate runs were performed.
The software-based analyses of the data obtained through thermogravimetry were based on an algorithm and the accompanying software noted that was previously reported [39,40,41]. The detailed kinetic analyses, including the mathematical treatment of the data, are also given in the above reports. In the present work, thermograms obtained at a relatively low heating rate of 10 °C min−1 were chosen for the analysis, as this is expected to capture most of the underlying steps in the thermal degradative pathway of the material in question. Essentially, the process involved the initial transfer of the raw data from the TGA instrument as an Excel file followed by processing, where the main step(s) of degradation of the sample were initially identified.

3. Results and Discussion

Generally, acrylic-based polymers are used as transparent plaques for various applications, where favourable optical clarity and enhanced weather resistance are the main prerequisites. In this context, the rigid solid materials casted from PSt-based materials are not sufficiently explored to date. However, for such applications, the relatively high flammability of PSt can become a limiting factor. Hence, in the present study, plaques of PSt were prepared (ca. 50 g scale) through the incorporation of various additives and reactives by adopting some procedures that were previously reported [11,33]. It is also relevant to note that the loading of phosphorus, in all cases, was normalized to 2 wt.%, while altering the chemical environments and oxidation states of the phosphorus atom in the admixtures. Furthermore, both the additive and reactive routes were utilized, with a view to identify the influences, if present, between the two strategies on the combustion features of the polymeric products. In addition, given the relatively nominal loading of phosphorus (2 wt.%), any marginal improvements in the fire retardance of the modified systems as compared to the virgin polymers would be most advantageous. The products obtained through the bulk polymerization route were chosen for further and detailed investigations in terms of their thermal (TGA) and calorimetric (DSC) properties, as well as their combustion (PCFC and ‘bomb’ calorimetry) characteristics. As previously reported, the final compositions of the products through the reactive strategy were effectively controlled with a high degree of certainty since the polymerization reactions were driven to near completion, i.e., ca. 99% conversion; the latter was established through 1H NMR spectra of the obtained plaques [34].
The bulk polymerization route employed in the present study for making PSt-based materials was found to be successful. In almost all cases, dense and tough polymeric plaques were formed. However, some exceptions were noted. The DOPO-modified version of PSt was found to be substantially brittle, and was also prone to shattering quite easily under a mechanical stress. Furthermore, the reactively modified version with the P- and N-containing comonomer, ADEPMAE, was found to have a plasticizing effect on the final product. The results obtained through the thermal and calorimetric evaluation of the products prepared through the bulk polymerization method are given, in detail, in the following sections.

3.1. Thermogravimetric Analysis (TGA)

In this section, the relevant TGA parameters obtained for each PSt-based sample at a heating rate of 10 °C min−1 are presented in Table 2, and the corresponding thermograms are given in Figure 1, Figure 2, Figure 3, Figure 4, Figure 5 and Figure 6, respectively. It is relevant to note here that, generally, the thermal degradation of PSt is strongly temperature-dependent [17]. For instance, at modest temperatures, initial cleavage occurs at a head-to-head linkage in the main chain, followed by smooth extrusion of styrene monomer, which, in fact, is the basis for recycling of the polymer. The TGA data obtained at 60 °C min−1 were primarily used for comparison with the relevant parameters obtained through the PCFC runs. The thermograms obtained for PSt samples generally exhibited only one main degradation step. However, during the initial phases of degradation, some small mass losses can be also observed in almost all the cases. Generally, the induction temperatures for the modified systems were noticeably lower than that of the unmodified version (Table 2). Furthermore, this effect was significantly higher in certain systems compared to others. On the other hand, the temperature at 50 wt.% was higher in the case of some of the modified systems than polystyrene.
As mentioned before, the induction temperatures seem to be lowered, albeit to varying degrees, in the modified systems as compared to the parent polymer. This could be either due to the release of the additives or early thermal cracking of the pendent P-containing groups prior to the onset of the main-chain decomposition of the polymer. Furthermore, the temperature at 50 wt.% mass loss were higher in several systems (DOPO, DEHPi, TEPi, TEPa, DEBP, and DEpVBP), indicating an enhanced resistance to mass loss as compared to unmodified PSt. However, in all other systems a reverse trend was observed, except in the case of the system incorporating TPP, where the corresponding temperature remained unaltered. The systems with the additive DEHPi and reactive P–N monomer (ADEPMAE), produced the maximum amounts of char (6.9 and 6.7 wt.%, respectively). Other components have also assisted in producing more char (except TPP), although to different extents.

3.2. Kinetic Analysis of the TGA Thermograms

The apparent values of the energy of activation (Ea) for PSt-based samples were obtained from the software runs [40]. It is relevant to note here that values quoted are averaged over the main decomposition step and the range of α values were also appropriately chosen. The results are collated in Table 3 below.
The virgin polymer was found to follow the kinetic model that was in conformance with first order (F1) kinetics (Ea value typically in the region of 180 to 220 kJ mol−1). Therefore, this particular model was subsequently applied in analysing all the modified versions of the styrene polymers. As in the case of PMMA samples [34], a reduction in the average activation energy values can be observed, except for the system containing the phosphite additive (DEHPi); here a relatively higher value (305 kJ mol−1) was obtained. Therefore, it is to be inferred here that, except in the case of DEHPi, in all other cases, the modification resulted in decreased thermal stability of the parent polymer.

3.3. Differential Scanning Calorimetry

Heats of pyrolysis (∆Hpyro) data and the values of the glass transition temperatures for various PSt-based bulk samples were obtained from the DSC runs of the samples at a heating rate of 10 °C min−1 in the temperature range of 30–550 °C. Given below are the results obtained for the PSt-based bulk samples from the DSC runs as well as their corresponding ∆Hpyro and Tg values (Table 4).
Here, a gradual decrease in the values of ∆Hpyro in the case of the modified materials can be observed, with the PSt+DEAEPa system exhibiting the lowest value of 324 mJ mg−1. Here, it can be assumed that in these systems, some degree of cooperative interaction between the polymeric matrix and the modifying groups are present during the phase changes that occur during a DSC run. It is also relevant to note that the modification with the phosphate comonomer DEAEPa showed the lowest values in both the systems. Furthermore, the modifications, in all cases, seem to lower the glass transition temperature as compared to the parent polymer matrix, which can be attributed to their varying plasticizing effects.

3.4. Pyrolysis Combustion Flow Calorimetry (PCFC)

The PCFC data of the PSt-based samples are shown below in Table 5.
From the above table it can be seen that all the modified versions have lower values of the relevant parameters, such as pHRR, THR, HRC, and EHC, when compared to the unmodified polystyrene sample. The material modified with the P–N monomer, ADEPMAE, shows the lowest values for pHRR (425 W g−1), THR (23.8 kJ g−1), HRC (424 J g−1 K−1), and EHC (25.2 kJ g−1), indicating that the modifying group has the most favourable effect amongst the systems under consideration [38,42]. It is also relevant to note that the char yields obtained for the different samples showed a wide variability, where no underlying trend can be found.
In addition, the first derivative of the TGA thermograms and HRR curves showed significant correspondence. Furthermore, all the polymeric systems showed a decreasing trend in the values of all the relevant parameters from the PCFC runs. This points towards the fact that when the modified versions of the PSt-based systems degrade, there appears to be a noticeable degree of cooperative interaction between the modifying groups and parent polymeric chains.

3.5. ‘Bomb’ Calorimetry

The values of the heat of combustion, ΔHcomb obtained through the ‘bomb’ calorimetric runs are collected in Table 6.
All the modified samples showed a definite decrease in the ∆Hcomb values as compared to the unmodified version, which clearly demonstrated the vapour-phase inhibitory effect(s) of the modifying groups. Such an effect was found to be particularly pronounced in the case of PSt modified with ADEPMAE, the P–N-containing monomer, where it may be also assumed that there is some degree of P–N interaction, thus exhibiting the lowest value of ∆Hcomb, 33.03 kJ g−1 [42]. It is also highly relevant to note here that, generally, there may be some sort of interaction (physical or chemical) of the parent polymer matrix with the modifying groups also evident during pyrolysis and combustion (from DSC and PCFC tests, respectively).

3.6. Some Generalizations among the Test Parameters

Some generalizations were found to exist amongst some of the relevant test parameters from TGA, PCFC, and ‘bomb’ calorimetry techniques. However, no particular correspondences were observed among the values of the char yields from the two techniques. However, several systems (such as unmodified PSt and modified versions with TPP, DEHPi, TEPi, DE-1-AEP, ADEPMAE, DEAEPa, and DEpVBP) showed substantial char residues (ranging from 3 to 8 wt.%) in the PCFC runs, whereas for the others the corresponding values closely resembled the char yield from the TGA runs (≤1 wt.%). Furthermore, several of the modifying additives and groups seem to exhibit some degree of condensed-phase activity during the PCFC runs. This was also evident in terms of enhanced char yields produced by the modified systems as compared to virgin PSt.
The relative values of ∆Hcomb and EHC did not show any particularly discernible trend and were varied amongst the samples. However, PSt containing the P–N monomer (ADEPMAE) exhibited significantly lower values, and in fact, its ∆Hcomb EHC values are particularly lower as compared to all other systems [42]. This, again, confirms the significant combustion inhibitory effect of the monomer as is also evident in the relevant parameters obtained through TGA, PCFC, and ‘bomb’ calorimetric techniques [42].

4. Conclusions

Through the present investigation on the thermal properties and combustion attributes of PSt-based polymers that were mainly obtained through TGA and calorimetric measurements (DSC, PCFC, and ‘bomb’ calorimetry), some inferences can be drawn: (1) TGA: Generally, the presence of additives or reactives in the parent polymer matrix was found to enhance its thermal stability. However, in the case of those systems containing the additives, there were no clear indications of the additives influencing the mode of degradation of the base polymeric matrix. It is relevant to note here that the degradation of the PSt base matrix is strongly influenced by the heating rate [43]; (2) DSC: Here, a gradual decrease in the values of ∆Hpyro in the case of all modified materials can be observed, with the PSt+DEAEPa system showing the lowest value. This can be attributed to the relative ease of volatilization and pyrolysis of the additive or reactive moieties as compared to the main-chain scission reaction of the parent polymeric matrix. Furthermore, the glass transition temperatures of the modified polymeric systems were noticeably lower than that of the unmodified counterpart. This can be attributed to the plasticizing effect of the additive compound and reactive group; (3) PCFC: All the modified versions showed lower values for the relevant parameters, such as pHRR, THR, HRC, and EHC, when compared to the unmodified polystyrene sample. The material modified with the P–N-monomer, ADEPMAE, showed the lowest values. Thus, these results point towards varying degrees of combustion inhibition in all the modified systems, presumably acting in the vapour phase; (4) ‘Bomb’ calorimetry: Here, the modified PSt-based samples showed a definite decrease in the ∆Hcomb values as compared to the unmodified version, which, again, clearly demonstrated the gaseous phase inhibitory effect(s) of the modifying groups. Such an effect was found to be particularly pronounced in the case of PSt modified with ADEPMAE, the P–N-containing monomer, where it can be also assumed that there is some degree of P–N interaction. The utility of the in-house developed software, in deducing the Arrhenius parameters from the TGA runs, was also explored and successfully applied, considering only a thermogram obtained through a single heating rate. The extended validity of these values should be treated with caution, and that such values can only be treated as ‘apparent’ values at best. The mode of action pertaining to P- and P–N-containing groups on the combustion attributes of the parent polymer matrix has been recently published [44].

Author Contributions

Conceptualization, P.J. and S.T.-M.; methodology, M.A., S.B., P.J. and S.T.-M.; investigation, M.A.; resources, S.B. and M.G.; data curation, M.A.; writing—original draft preparation, M.A. and S.B.; writing—review and editing, S.B., M.G. and P.J.; supervision, S.B., P.J. and S.T.-M.; project administration, P.J. and S.T.-M. All authors have read and agreed to the published version of the manuscript.

Funding

This research received no external funding.

Institutional Review Board Statement

Not applicable.

Informed Consent Statement

Not applicable.

Data Availability Statement

Not applicable.

Acknowledgments

One of us, M.A., is grateful to Victoria University, Melbourne, Australia, for the provision of a studentship.

Conflicts of Interest

The authors declare no conflict of interest.

References

  1. Lynwood, C. Polystyrene: Synthesis, Characteristics, and Applications; Nova Publishers: Hauppauge, NY, USA, 2014. [Google Scholar]
  2. Odian, G. Principles of Polymerization; John Wiley & Sons: Hoboken, NJ, USA, 2004. [Google Scholar]
  3. Atia, A.A.; Donia, A.M.; ELwakeel, K.Z. Adsorption behaviour of non-transition metal ions on a synthetic chelating resin bearing iminoacetate functions. Sep. Purif. Technol. 2005, 43, 43–48. [Google Scholar] [CrossRef]
  4. Atia, A.A.; Donia, A.M.; Elwakeel, K.Z. Selective separation of mercury (II) using a synthetic resin containing amine and mercaptan as chelating groups. React. Funct. Polym. 2005, 65, 267–275. [Google Scholar] [CrossRef]
  5. Donia, A.M.; Atia, A.A.; Elwakeel, K.Z. Gold (III) recovery using synthetic chelating resins with amine, thio and amine/mercaptan functionalities. Sep. Purif. Technol. 2005, 42, 111–116. [Google Scholar] [CrossRef]
  6. Elwakeel, K.Z.; Guibal, E. Potential use of magnetic glycidyl methacrylate resin as a mercury sorbent: From basic study to the application to wastewater treatment. J. Environ. Chem. Eng. 2016, 4, 3632–3645. [Google Scholar] [CrossRef]
  7. Sayadi, A.A.; Tapia, J.V.; Neitzert, T.R.; Clifton, G.C. Effects of expanded polystyrene (EPS) particles on fire resistance, thermal conductivity and compressive strength of foamed concrete. Constr. Build. Mater. 2016, 112, 716–724. [Google Scholar] [CrossRef]
  8. Price, D.; Cunliffe, L.K.; Bullett, K.; Hull, T.R.; Milnes, G.J.; Ebdon, J.R.; Hunt, B.J.; Joseph, P. Thermal behaviour of covalently bonded phosphate and phosphonate flame retardant polystyrene systems. Polym. Degrad. Stab. 2007, 92, 1101–1114. [Google Scholar] [CrossRef]
  9. Joseph, P.; Tretsiakova-McNally, S. Melt-flow behaviours of thermoplastic materials under fire conditions: Recent experimental studies and some theoretical approaches. Materials 2015, 8, 8793–8803. [Google Scholar] [CrossRef] [Green Version]
  10. Tiwari, A.; Raj, B. Reactions and Mechanisms in Thermal Analysis of Advanced Materials; John Wiley & Sons: Hoboken, NJ, USA, 2015. [Google Scholar]
  11. Ebdon, J.R.; Hunt, B.J.; Joseph, P.; Konkel, C.S.; Price, D.; Pyrah, K.; Hull, T.R.; Milnes, G.J.; Hill, S.B.; Lindsay, C.I. Thermal degradation and flame retardance in copolymers of methyl methacrylate with diethyl (methacryloyloxymethyl) phosphonate. Polym. Degrad. Stab. 2000, 70, 425–436. [Google Scholar] [CrossRef]
  12. McNeill, I.; Zulfiqar, M.; Kousar, T. A detailed investigation of the products of the thermal degradation of polystyrene. Polym. Degrad. Stab. 1990, 28, 131–151. [Google Scholar] [CrossRef]
  13. Jankowski, P.; Kedzierski, M. Synthesis of polystyrene of reduced flammability by suspension polymerization in the presence of halogen-free additives. Polimery 2011, 56, 20–26. [Google Scholar] [CrossRef]
  14. Cao, J.-P.; Zhao, X.; Zhao, J.; Zha, J.-W.; Hu, G.-H.; Dang, Z.-M. Improved thermal conductivity and flame retardancy in polystyrene/poly (vinylidene fluoride) blends by controlling selective localization and surface modification of SiC nanoparticles. ACS Appl. Mater. Interfaces 2013, 5, 6915–6924. [Google Scholar] [CrossRef] [PubMed]
  15. Edenharter, A.; Feicht, P.; Diar-Bakerly, B.; Beyer, G.; Breu, J. Superior flame retardant by combining high aspect ratio layered double hydroxide and graphene oxide. Polymer 2016, 91, 41–49. [Google Scholar] [CrossRef]
  16. Kausar, A.; Haider, S.; Muhammad, B. Nanocomposite based on polystyrene/polyamide blend and bentonite: Morphology, thermal, and nonflammability properties. Nanomater. Nanotechnol. 2017, 7, 1847980417702785. [Google Scholar] [CrossRef]
  17. Baby, A.; Tretsiakova-McNally, S.; Arun, M.; Joseph, P.; Zhang, J. Reactive and additive modifications of styrenic polymers with phosphorus-containing compounds and their effects on fire retardance. Molecules 2020, 25, 3779. [Google Scholar] [CrossRef] [PubMed]
  18. Gao, C.; Shi, Y.; Zhu, S.; Fu, L.; Feng, Y.; Lv, Y.; Yang, F.; Liu, M.; Shui, W. Induced assembly of polystyrene composites for simultaneously improving flame retardant and electromagnetic shielding properties. Polym. Adv. Technol. 2021, 32, 4251–4262. [Google Scholar] [CrossRef]
  19. Gao, C.; Shi, Y.; Chen, Y.; Zhu, S.; Feng, Y.; Lv, Y.; Yang, F.; Liu, M.; Shui, W. Constructing segregated polystyrene composites for excellent fire resistance and electromagnetic wave shielding. J. Colloid Interface Sci. 2022, 606, 1193–1204. [Google Scholar] [CrossRef] [PubMed]
  20. David, G.; Negrell-Guirao, C.; Iftene, F.; Boutevin, B.; Chougrani, K. Recent progress on phosphonate vinyl monomers and polymers therefore obtained by radical (co) polymerization. Polym. Chem. 2012, 3, 265–274. [Google Scholar] [CrossRef]
  21. Benin, V.; Cui, X.; Morgan, A.B.; Seiwert, K. Synthesis and flammability testing of epoxy functionalized phosphorous-based flame retardants. J. Appl. Polym. Sci. 2015, 132, 1–10. [Google Scholar] [CrossRef]
  22. Wang, K.; Morgan, A.B.; Benin, V. Preparation and studies of new phosphorus-containing diols as potential flame retardants. Fire Mater. 2017, 41, 973–982. [Google Scholar] [CrossRef]
  23. Costes, L.; Laoutid, F.; Brohez, S.; Dubois, P. Bio-based flame retardants: When nature meets fire protection. Mater. Sci. Eng. R Rep. 2017, 117, 1–25. [Google Scholar] [CrossRef]
  24. Hobbs, C.E. Recent advances in bio-based flame retardant additives for synthetic polymeric materials. Polymers 2019, 11, 224. [Google Scholar] [CrossRef] [PubMed] [Green Version]
  25. Mensah, R.A.; Shanmugam, V.; Narayanan, S.; Renner, J.S.; Babu, K.; Neisiany, R.E.; Försth, M.; Sas, G.; Das, O. A review of sustainable and environment-friendly flame retardants used in plastics. Polym. Test. 2022, 108, 107511. [Google Scholar] [CrossRef]
  26. Wilkie, C.A.; Morgan, A.B. Fire Retardancy of Polymeric Materials; CRC Press: Boca Raton, FL, USA, 2009. [Google Scholar]
  27. Ebdon, J.R.; Price, D.; Hunt, B.J.; Joseph, P.; Gao, F.; Milnes, G.J.; Cunliffe, L.K. Flame retardance in some polystyrenes and poly (methyl methacrylate) s with covalently bound phosphorus-containing groups: Initial screening experiments and some laser pyrolysis mechanistic studies. Polym. Degrad. Stab. 2000, 69, 267–277. [Google Scholar] [CrossRef]
  28. Joseph, P.; Tretsiakova-Mcnally, S. Reactive modifications of some chain-and step-growth polymers with phosphorus-containing compounds: Effects on flame retardance—A review. Polym. Adv. Technol. 2011, 22, 395–406. [Google Scholar] [CrossRef]
  29. Salmeia, K.A.; Gaan, S. An overview of some recent advances in DOPO-derivatives: Chemistry and flame retardant applications. Polym. Degrad. Stab. 2015, 113, 119–134. [Google Scholar] [CrossRef]
  30. Cullis, C.F.; Hirschler, M.M. The Combustion of Organic Polymers; Oxford University Press: London, UK, 1981; Volume 5. [Google Scholar]
  31. Joseph, P.; Ebdon, J.R. Recent developments in flame-retarding thermoplastics and thermosets. Fire Retard. Mater. 2000, 1, 220–263. [Google Scholar]
  32. Ebdon, J.; Bunt, B.; Joseph, P.; Konkel, C. Flame-retarding thermoplastics: Additive versus reactive approach. In Speciality Polymer Additives: Principles and Applications; John Wiley & Sons, Inc.: Hoboken, NJ, USA, 2001; pp. 231–257. [Google Scholar]
  33. Price, D.; Pyrah, K.; Hull, T.R.; Milnes, G.J.; Ebdon, J.R.; Hunt, B.J.; Joseph, P.; Konkel, C.S. Flame retarding poly (methyl methacrylate) with phosphorus-containing compounds: Comparison of an additive with a reactive approach. Polym. Degrad. Stab. 2001, 74, 441–447. [Google Scholar] [CrossRef]
  34. Arun, M.; Bigger, S.; Guerrieri, M.; Joseph, P. Thermal and calorimetric investigations of some phosphorus-modified chain growth polymers 1: Polymethyl methacrylate. Polymers 2022, 14, 1447. [Google Scholar] [CrossRef]
  35. Lyon, R.E.; Walters, R.N. Pyrolysis combustion flow calorimetry. J. Anal. Appl. Pyrolysis 2004, 71, 27–46. [Google Scholar] [CrossRef]
  36. Cogen, J.M.; Lin, T.S.; Lyon, R.E. Correlations between pyrolysis combustion flow calorimetry and conventional flammability tests with halogen-free flame retardant polyolefin compounds. Fire Mater. Int. J. 2009, 33, 33–50. [Google Scholar] [CrossRef]
  37. Sonnier, R.; Vahabi, H.; Ferry, L.; Lopez-Cuesta, J.-M. Pyrolysis-combustion flow calorimetry: A powerful tool to evaluate the flame retardancy of polymers. Fire Polym. VI New Adv. Flame Retard. Chem. Sci. 2012, 1118, 361–390. [Google Scholar]
  38. Tretsiakova-McNally, S.; Joseph, P. Pyrolysis combustion flow calorimetry studies on some reactively modified polymers. Polymers 2015, 7, 453–467. [Google Scholar] [CrossRef] [Green Version]
  39. Bigger, S.W.; Cran, M.J.; Bohn, M.A. Novel theoretical and computer-assisted modeling of isothermal and non-isothermal depolymerization kinetics. Polym. Test. 2015, 44, 1–7. [Google Scholar] [CrossRef]
  40. Bigger, S.W.; Cran, M.J.; Tawakkal, I.S. Two novel algorithms for the thermogravimetric assessment of polymer degradation under non-isothermal conditions. Polym. Test. 2015, 43, 139–146. [Google Scholar] [CrossRef]
  41. Thomas, A.; Moinuddin, K.; Tretsiakova-McNally, S.; Joseph, P. A kinetic analysis of the thermal degradation behaviours of some bio-based substrates. Polymers 2020, 12, 1830. [Google Scholar] [CrossRef]
  42. Joseph, P.; Tretsiakova-McNally, S. Combustion behaviours of chemically modified polyacrylonitrile polymers containing phosphorylamino groups. Polym. Degrad. Stab. 2012, 97, 2531–2535. [Google Scholar] [CrossRef]
  43. Faravelli, T.; Pinciroli, M.; Pisano, F.; Bozzano, G.; Dente, M.; Ranzi, E. Thermal degradation of polystyrene. J. Anal. Appl. Pyrolysis 2001, 60, 103–121. [Google Scholar] [CrossRef]
  44. Joseph, P.; Arun, M.; Bigger, S.; Guerrieri, M.; Pospiech, D.; Harnisch, C. Mode of action of condensed-and gaseous-phase fire retardation in some phosphorus-modified polymethyl methacrylate-and polystyrene-based bulk polymers. Polymers 2021, 13, 3402. [Google Scholar] [CrossRef]
Figure 1. An overlay of the TGA curves of the PSt-based materials with solid additives, at 10 °C min−1 in nitrogen, from 30 to 900 °C.
Figure 1. An overlay of the TGA curves of the PSt-based materials with solid additives, at 10 °C min−1 in nitrogen, from 30 to 900 °C.
Polymers 14 01520 g001
Figure 2. An overlay of the TGA curves of the PSt-based materials with liquid additives, at 10 °C min1 in nitrogen, from 30 to 900 °C.
Figure 2. An overlay of the TGA curves of the PSt-based materials with liquid additives, at 10 °C min1 in nitrogen, from 30 to 900 °C.
Polymers 14 01520 g002
Figure 3. An overlay of TGA curves of the PSt-based materials with reactives, at 10 °C min1 in nitrogen, from 30 to 900 °C.
Figure 3. An overlay of TGA curves of the PSt-based materials with reactives, at 10 °C min1 in nitrogen, from 30 to 900 °C.
Polymers 14 01520 g003
Figure 4. An overlay of the TGA curves of PSt and PSt+aliphatic phosphonate materials, at 10 °C min−1 in nitrogen, from 30 to 900 °C.
Figure 4. An overlay of the TGA curves of PSt and PSt+aliphatic phosphonate materials, at 10 °C min−1 in nitrogen, from 30 to 900 °C.
Polymers 14 01520 g004
Figure 5. An overlay of the TGA curves of PSt and PSt+aromatic phosphonate materials, at 10 °C min−1 in nitrogen, from 30 to 900 °C.
Figure 5. An overlay of the TGA curves of PSt and PSt+aromatic phosphonate materials, at 10 °C min−1 in nitrogen, from 30 to 900 °C.
Polymers 14 01520 g005
Figure 6. An overlay of the TGA curves of PSt and PSt+phosphate materials, at 10 °C min1 in nitrogen, from 30 to 900 °C.
Figure 6. An overlay of the TGA curves of PSt and PSt+phosphate materials, at 10 °C min1 in nitrogen, from 30 to 900 °C.
Polymers 14 01520 g006
Table 1. Details of the preparative data for St-based bulk polymers *.
Table 1. Details of the preparative data for St-based bulk polymers *.
Sl. No.Styrene (mL)Additive/ReactiveFormula WeightAdditive/Reactive Weight (g/mL)BPO/Dicumyl Peroxide (mg)
150.00---------50.0/25.0
236.57TPP2626.76 g44.0/22.0
336.10TPPO2787.17 g43.0/21.5
437.90DOPO2165.57 g43.0/21.5
540.09DEHPi1383.56 mL44.0/22.0
639.29TEPi1664.42 mL44.0/22.0
738.84TEPa1824.40 mL44.0/22.0
839.00DEPP1804.65 g44.0/22.0
937.53DEBP2285.88 g44.0/22.0
1023.32DE-1-AEP 2363.81 g26.0/13.0
1123.00ADPMAE 2654.27 g26.0/13.0
1223.00DEAEPa 2524.07 g26.0/13.0
1323.00DEpVBP 2544.10 g26.0/13.0
* since the pans were tightly stoppered during the curing phase, a near quantitative yield was obtained in each case (~99 wt.%).
Table 2. Some relevant parameters from the TGA analyses carried out in nitrogen at a heating rate of 10 °C min−1 of PSt-based systems.
Table 2. Some relevant parameters from the TGA analyses carried out in nitrogen at a heating rate of 10 °C min−1 of PSt-based systems.
Sl. No.SampleInduction Temp. (°C)Temp. at 50 wt.% (°C)Residue at 500 °C (wt.%)Final Residue at 800 °C (wt.%)
1Polystyrene1294080.50.4
2PSt+TPP1054080.20.0
3PSt+TPPO1234071.41.3
4PSt+DOPO1184201.00.8
5PSt+DEHPi73.04418.16.9
6PSt+TEPi75.04334.13.6
7PSt+TEPa1194241.82.1
8PSt+DEPP96.04070.90.9
9PSt+DEBP1004150.90.8
10PSt+DE-1-AEP1093904.93.6
11PSt+ADEPMAE72.03987.96.7
12PSt+DEAEPa74.03936.85.5
13PSt+DEpVBP1214374.94.0
Table 3. Energy of activation (Ea) and other relevant parameters of PSt-based samples obtained using the software (model: F1 First Order).
Table 3. Energy of activation (Ea) and other relevant parameters of PSt-based samples obtained using the software (model: F1 First Order).
Sl. No.SampleApparent Activation Energy (Ea, kJ mol−1)A (min−1)R2 Valuesα-Value Range
1PSt2702.68 × 10200.9980.1 to 0.9
2PSt+TPP1182.69 × 1080.91250.2 to 0.8
3PSt+TPPO1629.52 × 10110.97060.2 to 0.8
4PSt+DOPO1658.94 × 10110.99390.2 to 0.8
5PSt+DEHPi3051.23 × 10220.99430.1 to 0.9
6PSt+TEPi2293.88 × 10160.99080.2 to 0.8
7PSt+TEPa2102.24 × 10150.99350.2 to 0.8
8PSt+DEPP1573.82 × 10110.96520.2 to 0.8
9PSt+DEBP1376.79 × 1090.92180.2 to 0.8
10PSt+DE-1-AEP971.00 × 1070.98150.1 to 0.9
11PSt+ADEPMAE1303.82 × 1090.99780.4 to 0.9
12PSt+DEAEPa2164.26 × 10160.98710.2 to 0.8
13PSt+DEpVBP2231.08 × 10160.99230.2 to 0.8
Table 4. Heats of pyrolysis data of PSt-based materials obtained from DSC tests.
Table 4. Heats of pyrolysis data of PSt-based materials obtained from DSC tests.
Sl. No.SamplesHeats of Pyrolysis, ∆Hpyro (mJ mg−1)Tg (°C) (±5 °C)
1PSt81096
2PSt+TPP65055
3PSt+TPPO72076
4PSt+DOPO73061
5PSt+DEHPi54070
6PSt+TEPi56065
7PSt+TEPa68062
8PSt+DEPP69074
9PSt+DEBP66062
10PSt+DE-1-AEP56063
11PSt+ADEPMAE47070
12PSt+DEAEPa32465
13PSt+DEpVBP52075
Table 5. PCFC data of PSt-based materials.
Table 5. PCFC data of PSt-based materials.
Sl. No.SamplesTemp to pHRR (°C)pHRR (W g−1)THR (kJ g−1)HRC (J g−1 K−1)Char Yield (wt.%)EHC (kJ g−1)
1PSt43484037.18524.438.8
2PSt+TPP43468235.96866.538.4
3PSt+TPPO43471736.7729036.7
4PSt+DOPO44661836.3621036.3
5PSt+DEHPi46277832.97785.935
6PSt+TEPi46377131.97765.633.8
7PSt+TEPa44474334.2772034.2
8PSt+DEPP43881534.2813034.2
9PSt+DEBP44079234.5794034.5
10PSt+DE-1-AEP409501334997.435.6
11PSt+ADEPMAE43142523.84245.725.2
12PSt+DEAEPa41675731.97556.434.1
13PSt+DEpVBP46865534.66532.935.6
Table 6. Heats of combustion data for PSt-based samples from ‘bomb’ calorimetric measurements.
Table 6. Heats of combustion data for PSt-based samples from ‘bomb’ calorimetric measurements.
Sl. No.SampleΔHcomb (kJ g−1)
1PSt41.50
2PSt+TPP41.02
3PSt+TPPO 40.30
4PSt+DOPO 39.50
5PSt+DEHPi38.70
6PSt+TEPi 38.89
7PSt+TEPa38.99
8PSt+DEPP39.55
9PSt+DEBP39.13
10PSt+DE-1-AEP38.23
11PSt+ADEPMAE 33.03
12PSt+DEpVBP 39.47
The ∆Hcomb of PSt+DEAEPa could not be performed.
Publisher’s Note: MDPI stays neutral with regard to jurisdictional claims in published maps and institutional affiliations.

Share and Cite

MDPI and ACS Style

Arun, M.; Bigger, S.; Guerrieri, M.; Joseph, P.; Tretsiakova-McNally, S. Thermal and Calorimetric Investigations of Some Phosphorus-Modified Chain Growth Polymers 2: Polystyrene. Polymers 2022, 14, 1520. https://doi.org/10.3390/polym14081520

AMA Style

Arun M, Bigger S, Guerrieri M, Joseph P, Tretsiakova-McNally S. Thermal and Calorimetric Investigations of Some Phosphorus-Modified Chain Growth Polymers 2: Polystyrene. Polymers. 2022; 14(8):1520. https://doi.org/10.3390/polym14081520

Chicago/Turabian Style

Arun, Malavika, Stephen Bigger, Maurice Guerrieri, Paul Joseph, and Svetlana Tretsiakova-McNally. 2022. "Thermal and Calorimetric Investigations of Some Phosphorus-Modified Chain Growth Polymers 2: Polystyrene" Polymers 14, no. 8: 1520. https://doi.org/10.3390/polym14081520

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.

Article Metrics

Back to TopTop