Correction: Sapogova et al. Investigation of the Effect of Temperature Stabilization in Radiation–Heat Converters Based on a Strong Absorbing Coating. Photonics 2021, 8, 423
Previous Article in Special Issue
650 W All-Fiber Single-Frequency Polarization-Maintaining Fiber Amplifier Based on Hybrid Wavelength Pumping and Tapered Yb-Doped Fibers
 
 
Font Type:
Arial Georgia Verdana
Font Size:
Aa Aa Aa
Line Spacing:
Column Width:
Background:
Communication

Photo-Writable Sulfide Glasses Used to Fabricate Core-Clad Fiber Doped with Pr3+ for Mid-IR Luminescence

1
CNRS, ISCR-UMR 6226, Université Rennes, 35000 Rennes, France
2
Laboratoire de Physico-Chimie de l’Atmosphère, Université du Littoral-Côte d’Opale, 59140 Dunkerque, France
3
CIMAP, UMR 6252 CEA-CNRS-ENSICAEN, Université de Caen Normandie, 14050 Caen, France
*
Author to whom correspondence should be addressed.
Photonics 2022, 9(8), 549; https://doi.org/10.3390/photonics9080549
Submission received: 6 July 2022 / Revised: 1 August 2022 / Accepted: 2 August 2022 / Published: 5 August 2022
(This article belongs to the Special Issue Rare-Earth-Doped Fiber Lasers and Amplifiers)

Abstract

:
With the ultimate goal of developing rare-earth doped chalcogenide fiber fabrication for sensing, amplification, and laser applications, a core/clad germanium-gallium sulfide fiber doped with Pr3+ has been fabricated. The compositions of the core and the clad were selected to ensure the positive ∆n by adding CdI2 and CsCl, respectively, in the GeS2-Ga2S3 matrix. The choice of these compositions was also justified from experimental parameters, including characteristic temperatures and viscosity. Moreover, the permanent photo writability of the sulfide glass family by a femtosecond laser is investigated from the perspective of Bragg grating photo-inscription. Structural investigations by Raman spectroscopy are presented and the effect of the Pr3+ rare-earth ion on the structure is underlined. Finally, the emission of the step-index fiber, made by the rod-in-tube technique between 3.1 µm and 5.5 µm (by pumping at 1.55 µm), is demonstrated.

Introduction

The development of light sources in the mid-infrared range (MIR) has attracted increasing interest in the field of photonics over the last decade. As a matter of fact, they can find many areas of applications such as: (i) remote sensing for gases and chemical pollutants; (ii) medicine (since human tissues can be treated with MIR lasers); and (iii) national security and defense using MIR countermeasures. However, many of these applications in the MIR require compact and robust sources with an affordable price, high efficiency and output power, and good output beam quality.
In this context, up to now, only a few laser oscillations were observed in chalcogenide glass (ChG) fibers [1]. Over the last 25 years, several research teams have tried to obtain a laser action in the 3–5 µm spectral range. Nevertheless, the complexity and the difficulty of this fabrication of rare earth doped chalcogenide waveguides to obtain a laser gain are still present despite some very recent achievements [1]. One of the main causes lies firstly in the optical losses of a double index fiber at the excitation and the laser emission wavelengths. Second, the extrinsic non-radiative relaxations due to the presence of impurities, respectively, weaken the RE emission in the MIR. Recently, numerical simulations have provided new hopes and have been proposed as promising cascading lasing systems for Dy3+ doped chalcogenide fiber at 4.2 µm [2]. Subsequently, a MIR fiber laser based on Dy3+ doped sulfide glass was proposed [3]. Other papers relate the detailed theoretical study of laser amplification in Tb-doped chalcogenide fiber laser operating at 5.25 µm [4] or Pr-doped chalcogenide fibers pumped at 1.55 or 2 µm [5]. Analogously, a promising MIR laser numerical modeling was also developed in the case of Pr3+ doped ChG fiber [6,7].
Up to now, the most powerful fiber lasers realized in the MIR spectral range use ZBLAN fibers doped with RE ions [8]. The longest operating wavelength achieved is below 4.5 μm [9] due to the multiphonon relaxation in fluoride glasses that quenches the luminescence from higher energetic states. ChG have a lower phonon energy to achieve laser emission at longer wavelengths as demonstrated by calculations [10] and also possess a high refractive index, which is beneficial to obtain higher absorption and emission cross-sections in RE-doped glasses. Indeed, it should be noticed that laser emission up to 7.2 μm has been demonstrated in RE-doped halogenide crystal [11], but their high hygroscopicity makes them practically unusable (whereas this is not the case for ChG). The MIR luminescence of different RE in the ChG bulks or fibers for wavelengths beyond 4 µm has already been shown [12] and very recently a first MIR fiber lasing has been reported in the 5.1–5.2 µm range [13]. Nevertheless, up to now, the fabrication of a convenient MIR fiber laser in which the laser cavity will be directly embedded in the fiber core is not demonstrated yet. This last point requires for example the presence of Bragg mirrors (BM) inside the fiber core that could be inscribed by femtosecond laser writing. In other words, the composition of the ChG must allow simultaneously: (i) a femtosecond writing of the BM at the wavelength of inscription; and (ii) a high level of RE doping. The Ge-Ga-S glasses, which are transparent in the visible range, are suitable for laser writing at 800 nm [14]. The presence of gallium also facilitates the incorporation and the dispersion of RE ions by limiting the cluster formation [15]. The addition of metal halides in the glass composition facilitates the synthesis process and allows an adjustment of glass properties necessary to define the core and clad formulation. In this paper, we first investigate the effects on the thermal properties of CsCl and CdI2 addition in the glass matrix composition of [GeS2]0.80-[Ga2S3]0.20, and their behavior in terms of refractive index modification under femtosecond laser irradiations at 800 nm. This work is devoted to Raman structural analyses of the chosen clad and Pr3+-doped core compositions and to evaluating its emission performance.

2. Materials and Methods

2.1. Syntheses

The glasses from the systems ([GeS2]0.80-[Ga2S3]0.20)100-x-(CdI2)x and ([GeS2]0.80-[Ga2S3]0.20)100-x-(CsCl)x were synthesized from Ge (Umicore, 5 N), Ga (Alfa Aesar, 7 N), and S (Strem Chemicals, 5 N), as raw elements and from CdI2 (Alfa Aesar, 5 N) or CsCl (Alfa Aesar, 5N) compounds. The rare earth ions were added as Pr2S3 for the core glass doped with 1000 ppmw of Pr3+. The syntheses of the glasses were implemented by the melt-quenching method in a vacuum sealed silica set-up. The sulfur was distilled to remove traces of carbon, hydrogen, sulfide oxide, and water [16]. After homogenization of the molten liquid at 1023 K for several hours, the rods were obtained by quenching in water at room temperature and next an annealing at a temperature below the glass transition temperature (Tg), namely Tg-15 K [17]. The 7- or 10-mm diameter glass rods were then polished before their uses for the elaboration of fibers.

2.2. Thermal Characterizations

The glass transition temperatures (Tg) were determined by differential scanning calorimetric analyses on a DSC Q20 (Thermal Analysis Instrument). A sample mass of 5 to 10 mg was taken and introduced into an aluminum crucible which was then sealed and placed in the DSC furnace. Next, a temperature ramp of 10 K per minute was applied up to a maximum temperature of 773 K. For all compositions, no crystallization phenomenon was observable on the DSC traces.
The viscosity was measured by the parallel plate method on a Rheotronic® viscometer (Theta industries). A sample whose sides have been polished was placed between two plates. Then, a probe is placed on top with a constant pressure of 200 g. The glass is heated at a rate of 2 K·min−1 up to 823 K.
The thermal expansion coefficient α of the glasses was evaluated by thermomechanical analysis on a TMA 2940 dilatometer from the TA Instrument using Equation (1):
α = Δ L s L 0 T m a x T a m b
with ∆Ls is the sample length variation (mm), L0 is the sample length (mm) at room temperature, Tamb (K), and Tmax (K) is the maximal temperature of measurement. The measurement was performed up to Tg-10 K with a temperature rise rate of 2 K·min−1 under a constant pressure of 0.1 N.

2.3. Structural Characterizations

Raman scattering spectra are recorded for the two bulk glass compositions ([GeS2]0.80-[Ga2S3]0.20)90-(CsCl)10 and [GeS2]0.80-[Ga2S3]0.20)90-(CdI2)10:1000 ppm Pr3+ used as cladding and core glasses, respectively. A Horiba Scientific LabRAM HR Evolution spectrometer was used with a 785 nm laser diode as excitation source.

2.4. Step-Index Fiber Elabaration

The preforms were prepared by the rod-in-tube method. The composition ([GeS2]0.80-[Ga2S3]0.20)90-(CsCl)10 that was chosen for the clad was pierced and a rod of composition ([GeS2]0.80-[Ga2S3]0.20)90-(CdI2)10:1000 ppm Pr3+ was prepared for the core. In a recent paper, we have already determined the refractive indexes (n) of the glasses of these series. At similar x, the CdI2-based glasses possess a higher n [16]. In the chosen core and clad compositions, they are 2.074 and 2.039, respectively. The fibering process used to elaborate the step-index fiber has also been previously described in [16]. As a result, the preform was drawn into a 350 µm diameter core/cladding fiber with a core diameter of 60 µm.

2.5. Optical Characterizations

2.5.1. Femtosecond Laser ∆n Modification in the Glass Bulks

Usually, refractive index variations induced by femtosecond laser photo-inscription are carried out by translating the sample at constant speed, either parallel to the beam (longitudinal geometry) or perpendicular (transverse geometry). However, another methodology was applied in order to be consistent with the successful process used for the realization of optical components [18,19]. The inscriptions were made in a longitudinal geometry. In the first step, the beam was focused in the sample using a f = 50 mm lens and this one was irradiated during a time τ, by a pulse train of duration 250 fs with a repetition rate of 250 kHz, inducing the appearance of ∆n. The longitudinal displacement ∆z is about 10 µm. This value is chosen in order to obtain a good overlapping between the steps and then a good homogeneity of the resulting ∆n channel. These sequences were repeated for the entire length of the sample. Although the process is discontinuous, the resulting index variation is homogeneous.
The inscriptions were made in the bulk of the glass in pieces of dimensions 7 × 7 × 40 mm3. The samples were cut and polished into a 600 µm thickness plate before the evaluation of ∆n. Measurements of photo-induced index changes were performed by quantitative phase microscopy imaging [20] under a microscope with an X50 objective. On the other hand, we can notice that the longitudinal inscription geometry implies an axial symmetry of ∆n. Also, we can apply an inverse Abel transformation to the previous phase measurements in order to determine the profile of the index variation ∆n(r) [21]. We note that several measurements along the ∆n channel were made in order to verify the homogeneity of the results of the writing procedure.

2.5.2. Fluorescence Measurements

Fluorescence spectra were recorded using a diode emitting at 1.55 µm (Q-Photonics QSM 1550-3, Ann Arbor, USA) with incident power of 1030 mW, a liquid nitrogen cooled InSb detector adapted diffraction gratings for each wavelength domain and long-pass filter (Spectrogon LP-2500, Stockholm, Sweden) to remove any parasitic higher order contribution from the transmitted pump.

3. Results and Discussion

3.1. Thermal Properties

The evolutions of Tg as a function of the metal halide CsCl or CdI2 molar contents (x) are exhibited in Figure 1 for the glasses belonging to the two series ([GeS2]0.80-[Ga2S3]0.20)100-x-(CdI2)x and ([GeS2]0.80-[Ga2S3]0.20)100-x-(CsCl)x for 0 ≤ x ≤ 20. In both cases, a decrease of Tg is observed with the increase of x. This feature has mainly to be correlated to a dereticulation of the glass network due to the addition of halogens, which break the Ge-S or Ga-S bonds. More details on the structure of these glasses are given in the Section 3.3. Also, at constant metal halide molar content, the Tg difference between the CsCl- and CdI2-based glasses are never higher than 15 K. For example, at x = 10%, Tg are 668 K and 653 K for [GeS2]0.80-[Ga2S3]0.20)90-(CsCl)10 and [GeS2]0.80-[Ga2S3]0.20)90-(CdI2)10, respectively.
In addition, to shape a glass, the viscoplastic regime must show a viscosity between 108 and 103 Pa·s and its temperature range must be between Tg and the onset crystallization temperature Tx. In general, the fiber drawing for a chalcogenide glass is facilitated when the viscosity is below 106 Pa·s [22]. The temperature at which this level is reached gives an indication of the fiber drawing temperature. Figure 2a exhibits the evolution of the temperature for a viscosity of 106 Pa·s as a function of the molar content in metal halide. For glasses belonging to the two investigated series, this temperature monotonously decreases with x (and more pronouncedly for the CdI2-based glasses). This last observation has to be correlated to the halogen content, which is higher for CdI2- than for CsCl-based glasses at equal metal halide content. This trend is in good agreement with the decreasing Tg evolution as a function of x that is more important in the CdI2-based glasses (Figure 1). Moreover, Figure 2b shows that the thermal expansion coefficient (α) increases with the metal halide content for the series based on CsCl, while it remains almost constant for the series containing CdI2. Indeed, α grows from 10 × 10−6 K−1 up to 26 × 10−6 K−1 for x equal to 5 and 20 in CsCl-based glasses, respectively, whereas it stagnates around 9.5 × 10−6 K−1 for CdI2-based glasses. These features can be attributed to the size of the cations since, according to Pauling radii, the ionic radii of Cs+ and Cd2+ are 1.69 Å and 0.97 Å, respectively.
The data in Table 1 allow us to compare the thermal characteristics of the composition of the fiber core undoped and Pr3+-doped. The addition of praseodymium does not significantly influence the thermal properties, meaning that the behavior of the doped glass during the drawing process will probably remain unchanged.

3.2. Refractive Index Modification by Femtosecond Laser

In our study, two types of experiments are presented. In the first one, shown in Figure 3a, the average beam power is fixed (P = 20 mW) and the duration of the pulse burst τ varies. In the second case, Figure 3b, τ is fixed at 100 ms and the study focuses on the influence of the incident power. The results are quite similar in both series for the 2 experiments. First of all, when P is fixed at 20 mW, the generated ∆n reach 6.10−3 for a duration pulse higher than 125 ms. Next, for τ = 100 ms, a threshold appears around 10 mW. Below this power the ∆n is negligible, whilst above 15 mW it reaches 6.10−3. Finally, the previous works published elsewhere [14,19] and the present studies of refractive index modification by femtosecond laser allow us to positively consider this technique for inscribing BM inside the core of the fiber.

3.3. Glass Structure

The Raman spectra of [GeS2]0.80-[Ga2S3]0.20)90-(CsCl)10 and [GeS2]0.80-[Ga2S3]0.20)90-(CdI2)10:1000 ppmw Pr3+ bulk glasses are dominated, as can be seen in Figure 4, by the presence of a band at 340 cm−1 and a shoulder observed at 370 cm−1. These band and shoulder correspond to the symmetric ν1(A1) stretching modes of the [GeS4] tetrahedra[23] bound by their corners and to the companion mode of the ν1 symmetric streching modes related to vibrations of the [GeS4] tetrahedra linked by their edges. A band at 430 cm−1 is assigned to vibrations of S3Ge-S-GeS3 units where the tetrahedra are connected by their corners and the asymmetric streching mode of [GeS4] tetrahedra is expected to present a moderate contribution at 385–405 cm−1. A broadening of the dominant peak is associated with the presence of gallium in Ge-based glass, which can be attributed to the symmetric stretching mode of [GaS4] tetrahedra (around 320–350 cm−1), usually accompanied by S3Ga-S-GaS3 units around 360–390 cm−1 [24,25,26,27,28]. In case of a deficit in sulfur in glass composition, a triscluster of [GaS4] sharing one S tricoordinated as in the case of α-Ga2S3 crystal, was also proposed and calculated from the density functional theory (DFT) simulation at 315 and 397 cm−1 or 325 cm−1 without clear attribution in experimental Raman spectrum [29,30]. The possible presence of an edge-sharing (ES) [GaS4] unit was proposed to present vibration at 240 cm−1 [29] or 270 cm−1 of two edge-shared tetrahedra [31]. The band located at 474 cm−1 attributed to the stretching vibrational modes of homopolar S-S bonds, which can form dimers, small chains, or S8 rings is only very weakly present in ([GeS2]0.80-[Ga2S3]0.20)90-(CsCl)10 and ([GeS2]0.80-[Ga2S3]0.20)90-(CdI2)10:1000 ppm Pr3+ from Pr2Se3. The presence of CsCl in Ge-Ga-S seems to have a not very pronounced impact on the whole of the spectrum, probably causing a broadening of bands with really spread contributions over the whole of the spectrum and generally related to an insertion of chlorine in the entities tetrahedral via a substitution of S by Cl. On the other hand, we note a retively noticeable difference on the bands between 240 and 270 cm1 between the CsCl and CdI2 glasses. A small band is observed at 270 cm−1 for ([GeS2]0.80-[Ga2S3]0.20)90-(CsCl)10 and additionaly, a weak shoulder at 258 cm−1 and a medium band at 240 cm−1 for ([GeS2]0.80-[Ga2S3]0.20)90-(CdI2)10. In this spectral range, the vibration mode of S3Ga-Ge(Ga)S3 can be expected around 268 cm−1, for which it is difficult to distinguish Ge-Ga bonds from Ga-Ga bonds due to their very close atomic weight. The band at 240 cm−1 is already observed as a clear shoulder of the 270 cm−1 band in Na2S-Ga2S3-CsCl and GeS2-Ga2S3 glasses when Ga2S3 increased and could be related to vibration of two edge-shared [GaS4] tetrahedra or [Gay-GaS4-y]. The shoulder may be associated with the vibrational modes of Ge-Ge homopolar bonds (likely at 258 cm−1) existing in the S3Ge-GeS3 ethane-type units or [Gey-GeS4-y] for sulfur-deficient Ge-based glasses. It was also reported in GeS2- CdI2 and GeS2-Ga2S3-CdI2 glasses the presence of a double band at 240 cm−1 and 258 cm−1 which clearly increases with increasing CdI2. This could be related to the presence of two edge-shared [GaS4] tetrahedra or [Gay-GaS4−y] and S3Ge-GeS3 in greater proportion but it is also proposed that the presence of both [GaS3I] and [GeS3I] are susceptible to the present contribution.

3.4. MIR Emission of Core-Clad Sulfide Fiber

First of all, the optical losses of the double index fiber ([GeS2]0.80-[Ga2S3]0.20)90-(CsCl)10 and ([GeS2]0.80-[Ga2S3]0.20)90-(CdI2)10:1000 ppmw Pr3+ have been estimated by the cut-back method. Typically, these optical losses are about a few tens of dB.m1 between 2.5 and 8 µm. Even if this characteristic is not satisfactory, the emission spectrum of the core of the doped step-index fiber was still measured. A broad emission band is, as expected, observed in the 3.2 to 5.5 µm spectral range (Figure 5a). This emission band is related to the transitions (3F2, 3H6) → 3H5 (3.5–4.2 µm) and 3H53H4 (4.0–5.5 µm), as shown in Figure 5b. The radiative emission centered at 4 µm is clearly present but the one normally centered at 5.2 µm is not visible, mainly due to parasitic absorptions (and likely due to C-S bonds). The 3.2 µm band from the second harmonic of the pump is still visible (although attenuated by a filter) and the absorption peak at 4.2 µm is caused by CO2.
The first fluorescence spectrum obtained in this double index fiber is encouraging despite the low intensity produced related to important optical losses. A new method of improvement in the synthesis of the glass and in the design of the fiber may soon be envisaged for this composition in order to considerably reduce these optical losses and to increase the intensity of their emission.

4. Conclusions

The synthesis and the characterizations of glasses belonging to the series ([GeS2]0.80-[Ga2S3]0.20)100-x-(CsCl)x and ([GeS2]0.80-[Ga2S3]0.20)100-x-(CdI2)x have been implemented. Thermal properties have been studied and the photo-writability of the chosen core and clad compositions by femtosecond laser have been demonstrated. As a first step toward an MIR fiber laser, a step index fiber with a photo-writable core doped with Pr3+ ions has been elaborated. The Pr3+-doped double index fiber thus produced has allowed a MIR radiation around 4 µm. At this stage, even if the results are very promising, some improvements in the synthesis and fibering process will be necessary to reduce the optical losses and then to increase the level of emission before considering a fiber laser effect.

Author Contributions

Conceptualization, J.C., J.T., and D.L.C.; methodology, J.C., C.B.-P., F.S., and A.B.; formal analysis, P.M., and V.N.; investigation, J.C., F.S., P.M., and V.N.; writing—original draft preparation, J.C.; writing—review and editing, D.L.C., V.N., and P.C.; funding acquisition, J.T., and D.L.C. All authors have read and agreed to the published version of the manuscript.

Funding

This research was funded by Agence Nationale de la Recherche (ANR, France), grant number ANR-17-CE24-0002-02 corresponding to the COMI project.

Institutional Review Board Statement

Not applicable.

Informed Consent Statement

Not applicable.

Data Availability Statement

The data that support the plots within this paper are available from the corresponding author on request.

Acknowledgments

Julie Carcreff acknowledges both the French Agence de l’Innovation pour la Défense (AID) and the Agence Nationale de la Recherche (ANR, France) for the PhD financial supports. Platform Spectroscopy Infrared and Raman (SIR – ScanMAT, Université de Rennes 1) is acknowledged for performed Raman measurements.

Conflicts of Interest

The authors declare no conflict of interest related to this article.

References

  1. Nazabal, V.; Adam, J.-L. Infrared Luminescence of Chalcogenide Glasses Doped with Rare Earth Ions and Their Potential Applications. Opt. Mater. X 2022, 15, 100168. [Google Scholar] [CrossRef]
  2. Cui, J.; Xiao, X.; Xu, Y.; Cui, X.; Chen, M.; Guo, J.; Lu, M.; Peng, B.; Guo, H. Mid-Infrared Emissions of Dy3+ Doped Ga-As-S Chalcogenide Glasses and Fibers and Their Potential for a 4.2 Μm Fiber Laser. Opt. Mater. Express 2018, 8, 2089–2102. [Google Scholar] [CrossRef]
  3. Falconi, M.C.; Palma, G.; Starecki, F.; Nazabal, V.; Troles, J.; Adam, J.L.; Taccheo, S.; Ferrari, M.; Prudenzano, F. Dysprosium-Doped Chalcogenide Master Oscillator Power Amplifier (MOPA) for Mid-IR Emission. J. Light. Technol. 2017, 35, 265–273. [Google Scholar] [CrossRef] [Green Version]
  4. Denker, B.I.; Galagan, B.I.; Koltashev, V.V.; Plotnichenko, V.G.; Snopatin, G.E.; Sukhanov, M.V.; Sverchkov, S.E.; Velmuzhov, A.P. Continuous Tb-Doped Fiber Laser Emitting at ∼5.25 Μm. Opt. Laser Technol. 2022, 154, 108355. [Google Scholar] [CrossRef]
  5. Anashkina, E.A.; Kim, A.V. Numerical Simulation of Ultrashort Mid-IR Pulse Amplification in Praseodymium-Doped Chalcogenide Fibers. J. Light. Technol. 2017, 35, 5397–5403. [Google Scholar] [CrossRef]
  6. Sójka, L.; Tang, Z.; Furniss, D.; Sakr, H.; Bereś-Pawlik, E.; Seddon, A.B.; Benson, T.M.; Sujecki, S. Numerical and Experimental Investigation of Mid-Infrared Laser Action in Resonantly Pumped Pr3+ Doped Chalcogenide Fibre. Opt. Quantum Electron. 2017, 49, 21. [Google Scholar] [CrossRef] [Green Version]
  7. Churbanov, M.F.; Denker, B.I.; Galagan, B.I.; Koltashev, V.V.; Plotnichenko, V.G.; Snopatin, G.E.; Sukhanov, M.V.; Sverchkov, S.E.; Velmuzhov, A.P. Laser Potential of Pr3+ Doped Chalcogenide Glass in 5-6 Μm Spectral Range. J. Non Cryst. Solids 2021, 559, 120592. [Google Scholar] [CrossRef]
  8. Maes, F.; Fortin, V.; Poulain, S.; Poulain, M.; Carrée, J.-Y.; Bernier, M.; Vallée, R. Room-Temperature Fiber Laser at 3.92 Μm. Optica 2018, 5, 761–764. [Google Scholar] [CrossRef]
  9. Sujecki, S. Modelling and Design of Lanthanide Ion Doped Chalcogenide Fiber Lasers: Progress towards the Practical Realization of the First MIR Chalcogenide Fiber Laser. Fibers 2018, 6, 25. [Google Scholar] [CrossRef] [Green Version]
  10. Karaksina, E.V.; Kotereva, T.V.; Shiryaev, V.S. Luminescence Properties of Core-Clad Pr-Doped Ge-As-Se-Ga(In,I) Glass Fibers. J. Lumin. 2018, 204, 154–156. [Google Scholar] [CrossRef]
  11. Bowman, S.R.; Shaw, L.B.; Feldman, B.J.; Ganem, J. A 7-Μm Praseodymium-Based Solid-State Laser. IEEE J. Quantum Electron. 1996, 32, 646–649. [Google Scholar] [CrossRef]
  12. Chahal, R.; Starecki, F.; Doualan, J.-L.; Němec, P.; Trapananti, A.; Prestipino, C.; Tricot, G.; Boussard-Pledel, C.; Michel, K.; Braud, A.; et al. Nd3+: Ga-Ge-Sb-S Glasses and Fibers for Luminescence in Mid-IR: Synthesis, Structural Characterization and Rare Earth Spectroscopy. Opt. Mater. Express 2018, 8, 1650. [Google Scholar] [CrossRef]
  13. Nunes, J.J.; Sojka, Ł.; Crane, R.W.; Furniss, D.; Tang, Z.Q.; Tang, Z.Q.; Mabwa, D.; Xiao, B.; Benson, T.M.; Farries, M.; et al. Room Temperature Mid-Infrared Fiber Lasing beyond 5 Μm in Chalcogenide Glass Small-Core Step Index Fiber. Opt. Lett. 2021, 46, 3504–3507. [Google Scholar] [CrossRef] [PubMed]
  14. Caulier, O.; Le Coq, D.; Calvez, L.; Bychkov, E.; Masselin, P. Free Carrier Accumulation during Direct Laser Writing in Chalcogenide Glass by Light Filamentation. Phys. A Mater. Sci. Process 2011, 77, 109–111. [Google Scholar] [CrossRef] [PubMed]
  15. Aitken, B.G.; Quimby, R.S. Rare-Earth-Doped Multicomponent Ge-Based Sulphide Glasses. J. Non Cryst. Solids 1997, 213–214, 281–287. [Google Scholar] [CrossRef]
  16. Carcreff, J.; Masselin, P.; Boussard-Plédel, C.; Kulinski, P.; Troles, J.; Le Coq, D. Step-Index Fibre from Metal Halide Chalcogenide Glasses. Opt. Mater. Express 2020, 10, 2800. [Google Scholar] [CrossRef]
  17. Ledemi, Y.; Bureau, B.; Calvez, L.; Le Floch, M.; Rozé, M.; Lin, C.; Zhang, X.H.; Allix, M.; Matzen, G.; Messaddeq, Y. Structural Investigations of Glass Ceramics in the Ga2S3-GeS2-CsCl System. J. Phys. Chem. B 2009, 113, 14574–14580. [Google Scholar] [CrossRef]
  18. Masselin, P.; Bychkov, E.; Le Coq, D. Direct Laser Writing of a Low-Loss Waveguide with Independent Control over the Transverse Dimension and the Refractive Index Contrast between the Core and the Cladding. Opt. Lett. 2016, 41, 3507. [Google Scholar] [CrossRef]
  19. Masselin, P.; Bychkov, E.; Le Coq, D. Ultrafast Laser Inscription of High-Performance Mid-Infrared Waveguides in Chalcogenide Glass. IEEE Photonics Technol. Lett. 2018, 30, 2123–2126. [Google Scholar] [CrossRef] [Green Version]
  20. Barty, A.; Roberts, A.; Paganin, D.; Nugent, K.A. Quantitative Optical Phase Microscopy. Opt. Lett. 1998, 23, 817–819. [Google Scholar] [CrossRef]
  21. Ampem-Lassen, E.; Huntington, S.T.; Dragomir, N.M.; Nugent, K.A.; Roberts, A. Refractive Index Profiling of Axially Symmetric Optical Fibers: A New Technique. Opt. Express 2005, 13, 3277. [Google Scholar] [CrossRef] [PubMed]
  22. Yang, G.; Rouxel, T.; Troles, J.; Bureau, B.; Boussard-Plédel, C.; Houizot, P.; Sangleboeuf, J.C. Viscosity of As2Se3 Glass During the Fiber Drawing Process. J. Am. Ceram. Soc. 2011, 94, 2408–2411. [Google Scholar] [CrossRef]
  23. Lucovsky, G.; Deneufville, J.P.; Galeener, F.L. Study of the Optic Modes of Ge0.30S0.70 Glass by Infrared and Raman Spectroscopy. Phys. Rev. B 1974, 9, 1591–1597. [Google Scholar] [CrossRef]
  24. Julien, C.; Barnier, S.; Massot, M.; Chbani, N.; Cai, X.; Loireau-Lozac’h, A.M.; Guittard, M. Raman and Infrared Spectroscopic Studies of Ge-Ga-Ag Sulphide Glasses. Mater. Sci. Eng. B 1994, 22, 191–200. [Google Scholar] [CrossRef]
  25. Pethes, I.; Chahal, R.; Nazabal, V.; Prestipino, C.; Trapananti, A.; Pantalei, C.; Beuneu, B.; Bureau, B.; Jóvári, P. Short Range Order in Ge-Ga-Se Glasses. J. Alloys Compd. 2015, 651, 578–584. [Google Scholar] [CrossRef]
  26. Pethes, I.; Nazabal, V.; Chahal, R.; Bureau, B.; Kaban, I.; Belin, S.; Jóvári, P. Local Motifs in GeS2–Ga2S3 Glasses. J. Alloys Compd. 2016, 673, 149–157. [Google Scholar] [CrossRef] [Green Version]
  27. Ishibashi, T.; Takebe, H.; Morinaga, K. Glass Forming Region and Structure of Vitreous RS-Ga2S3(R=Ca, Sr, Ba). J. Ceram. Soc. Jpn. 2003, 111, 308–311. [Google Scholar] [CrossRef] [Green Version]
  28. Heo, J.; Yoon, J.M.; Ryou, S.Y. Raman Spectroscopic Analysis on the Solubility Mechanism of La3+ in GeS2–Ga2S3 Glasses. J. Non Cryst. Solids 1998, 238, 115–123. [Google Scholar] [CrossRef]
  29. Cuisset, A.; Hindle, F.; Laureyns, J.; Bychkov, E. Structural Analysis of XCsCl(1−x)Ga2S3 Glasses by Means of DFT Calculations and Raman Spectroscopy. J. Raman Spectrosc. 2010, 41, 1050–1058. [Google Scholar] [CrossRef]
  30. Masselin, P.; Le Coq, D.; Cuisset, A.; Bychkov, E. Spatially Resolved Raman Analysis of Laser Induced Refractive Index Variation in Chalcogenide Glass. Opt. Mater. Express 2012, 2, 1768. [Google Scholar] [CrossRef]
  31. Barbosa, L.C.; Cesar, C.L.; Mazali, I.O.; Alves, O.L. Spectroscopic and Thermal Properties of Ga2S3–Na2S–CsCl Glasses. J. Am. Ceram. Soc. 2006, 89, 1037–1041. [Google Scholar] [CrossRef]
Figure 1. Evolution of Tg as a function the metal halide CsCl (blue crosses) or CdI2 (red squares) content. Inset correspond to the DSC traces of glasses with 10 mol. % of CsCl (blue line) or CdI2 (red line).
Figure 1. Evolution of Tg as a function the metal halide CsCl (blue crosses) or CdI2 (red squares) content. Inset correspond to the DSC traces of glasses with 10 mol. % of CsCl (blue line) or CdI2 (red line).
Photonics 09 00549 g001
Figure 2. (a) Evolution of the measured temperature at a viscosity of 106 Pa·s as a function the metal halide CsCl (blue crosses) or CdI2 (red squares) content. (b) Evolution of the thermal expansion coefficient as a function the metal halide CsCl (blue crosses) or CdI2 (red squares) content.
Figure 2. (a) Evolution of the measured temperature at a viscosity of 106 Pa·s as a function the metal halide CsCl (blue crosses) or CdI2 (red squares) content. (b) Evolution of the thermal expansion coefficient as a function the metal halide CsCl (blue crosses) or CdI2 (red squares) content.
Photonics 09 00549 g002
Figure 3. Evolution of the refractive index modification (∆n) as a function of (a) the irradiation time (τ) at 20 mW and (b) the average power (P) and the corresponding intensity with τ = 100 ms in the selected glasses for the step-index fiber (CsCl—(blue cross) and CdI2—(red square) based glasses.
Figure 3. Evolution of the refractive index modification (∆n) as a function of (a) the irradiation time (τ) at 20 mW and (b) the average power (P) and the corresponding intensity with τ = 100 ms in the selected glasses for the step-index fiber (CsCl—(blue cross) and CdI2—(red square) based glasses.
Photonics 09 00549 g003
Figure 4. Raman spectra of the glasses ([GeS2]0.80-[Ga2S3]0.20)90-(CsCl)10 and ([GeS2]0.80-[Ga2S3]0.20)90-(CdI2)10:1000 ppmw Pr3+ recorded at 785 nm.
Figure 4. Raman spectra of the glasses ([GeS2]0.80-[Ga2S3]0.20)90-(CsCl)10 and ([GeS2]0.80-[Ga2S3]0.20)90-(CdI2)10:1000 ppmw Pr3+ recorded at 785 nm.
Photonics 09 00549 g004
Figure 5. (a) Fluorescence intensity of the core of the double index fiber glasses ([GeS2]0.80-[Ga2S3]0.20)90-(CsCl)10 and ([GeS2]0.80-[Ga2S3]0.20)90-(CdI2)10:1000 ppmw Pr3+) as a function of the wavelength; (b) energy level diagram of ion Pr3+.
Figure 5. (a) Fluorescence intensity of the core of the double index fiber glasses ([GeS2]0.80-[Ga2S3]0.20)90-(CsCl)10 and ([GeS2]0.80-[Ga2S3]0.20)90-(CdI2)10:1000 ppmw Pr3+) as a function of the wavelength; (b) energy level diagram of ion Pr3+.
Photonics 09 00549 g005
Table 1. Thermal characteristics of glasses corresponding to the undoped and Pr3+-doped cores, [GeS2]0.80-[Ga2S3]0.20)90-(CdI2)10 and [GeS2]0.80-[Ga2S3]0.20)90-(CdI2)10:1000 ppmw Pr3+, respectively.
Table 1. Thermal characteristics of glasses corresponding to the undoped and Pr3+-doped cores, [GeS2]0.80-[Ga2S3]0.20)90-(CdI2)10 and [GeS2]0.80-[Ga2S3]0.20)90-(CdI2)10:1000 ppmw Pr3+, respectively.
Glass CompositionTg (K) ± 2 KTx (K) ± 2 K∆T (K) ± 4 Kα (10−6 K−1) ± 0.5 × 10−6 K−1T at 106 Pa·s ± 2 K
Undoped core653>773>12010.1728
Pr3+-doped core654 >773>11910.5730
Publisher’s Note: MDPI stays neutral with regard to jurisdictional claims in published maps and institutional affiliations.

Share and Cite

MDPI and ACS Style

Carcreff, J.; Nazabal, V.; Troles, J.; Boussard-Plédel, C.; Masselin, P.; Starecki, F.; Braud, A.; Camy, P.; Le Coq, D. Photo-Writable Sulfide Glasses Used to Fabricate Core-Clad Fiber Doped with Pr3+ for Mid-IR Luminescence. Photonics 2022, 9, 549. https://doi.org/10.3390/photonics9080549

AMA Style

Carcreff J, Nazabal V, Troles J, Boussard-Plédel C, Masselin P, Starecki F, Braud A, Camy P, Le Coq D. Photo-Writable Sulfide Glasses Used to Fabricate Core-Clad Fiber Doped with Pr3+ for Mid-IR Luminescence. Photonics. 2022; 9(8):549. https://doi.org/10.3390/photonics9080549

Chicago/Turabian Style

Carcreff, Julie, Virginie Nazabal, Johann Troles, Catherine Boussard-Plédel, Pascal Masselin, Florent Starecki, Alain Braud, Patrice Camy, and David Le Coq. 2022. "Photo-Writable Sulfide Glasses Used to Fabricate Core-Clad Fiber Doped with Pr3+ for Mid-IR Luminescence" Photonics 9, no. 8: 549. https://doi.org/10.3390/photonics9080549

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.

Article Metrics

Back to TopTop