Next Article in Journal
Interlaminar Shear Characteristics, Energy Consumption, and Carbon Emissions of Polyurethane Mixtures
Next Article in Special Issue
Evaluation of Infiltrant Application in the Course of Root Cementum Caries with Different Methods of Surface Preparation—An In Vitro Study
Previous Article in Journal
Surface Modification of Polyester/Viscose Fabric with Silica Hydrosol and Amino-Functionalized Polydimethylsiloxane for the Preparation of a Fluorine-Free Superhydrophobic and Breathable Textile
Previous Article in Special Issue
The Cytotoxicity of OptiBond Solo Plus and Its Effect on Sulfur Enzymes Expression in Human Fibroblast Cell Line Hs27
 
 
Font Type:
Arial Georgia Verdana
Font Size:
Aa Aa Aa
Line Spacing:
Column Width:
Background:
Article

The Effect of Different Surface Conditioning Techniques on the Bonding between Resin Cement & Ceramic

1
Department of Prosthetic Dental Science, College of Dentistry, Jazan University, Jazan 45142, Saudi Arabia
2
Department of Maxillofacial Surgery and Diagnostic Sciences, Division of Oral Pathology, College of Dentistry, Jazan University, Jazan 45142, Saudi Arabia
3
Department of Prosthodontics, Swargiya Dadasaheb Kalmegh Smruti Dental College & Hospital, Nagpur 441110, India
4
Department of Restorative Science, College of Dentistry, Riyadh Elm University, Riyadh 12611, Saudi Arabia
5
Department of Conservative Dental Sciences, College of Dentistry, Prince Sattam bin Abdulaziz University, Alkharj 16273, Saudi Arabia
6
Department of Restoratives Science, King Abdulaziz University, Jeddah 21589, Saudi Arabia
7
Department of Restorative Dental Science, King Khalid University, Abha 61421, Saudi Arabia
8
Centre of Molecular Medicine and Diagnostics (COMManD), Department of Biochemistry, Saveetha Dental College & Hospitals, Saveetha Institute of Medical and Technical Sciences, Saveetha University, Chennai 600077, India
9
Department of Restorative Dental Sciences, College of Dentistry, Jazan University, Jazan 45142, Saudi Arabia
10
Department of Oral Pathology and Microbiology, Sri Venkateswara Dental College and Hospital, Chennai 600130, India
*
Author to whom correspondence should be addressed.
Coatings 2022, 12(3), 399; https://doi.org/10.3390/coatings12030399
Submission received: 19 January 2022 / Revised: 11 March 2022 / Accepted: 12 March 2022 / Published: 17 March 2022
(This article belongs to the Special Issue Advances and Innovations in Dental Materials and Coatings)

Abstract

:
Surface etching before cementation is a vital step that determines the clinical performance of ceramic restorations. Etching alters surface topography that contributes effective bonding between ceramic restoration and resin cement. This study aimed to compare etching techniques to determine the most effective etching method contributing the highest bond strength that helps in improving dental implants. Materials and methods: sixty discs of feldspathic ceramic measuring 10 mm diameter and 4 mm thickness were prepared. The 60 samples were divided into four equal groups based on the surface treatment technique used: group A: 9.6% hydrofluoric acid; group B: coarse diamond burs; group C: CO2 laser; and group D: no treatment. Ceramic disc specimens were examined under a Scanning Electron microscope (SEM) after surface treatment to characterize their surface morphology. Further, the specimens were luted with a resin luting agent and incubated for 24 h at a temperature of 37 °C simulating the oral environment. After 24 h, shear bond strength (SBS) and the nature of bond failure was determined for each specimen using a universal Instron testing machine. Results: significant change in surface morphology was noticed on hydrofluoric acid treatment forming larger irregular roughness (4.83 ± 1.78 µm) with multiple patterns of grooves and pores compared to other groups. Further, the highest SBS value was measured on hydrofluoric acid etching that display the highest bond strength due to the high surface roughness. In conclusion, our findings report a strong association between the surface roughness and bond strength upon hydrofluoric acid compared to other methods. Further work in this direction will enhance the utility of the etching technique on the improvement of dental implants.

1. Introduction

Dental porcelains are ideally suited for anterior esthetic restorations. Their color stability, resistance to staining, wear-resistance, and biocompatibility allow it to simulate natural teeth structure [1]. Their favourable esthetics combined with a conservative tooth preparation make them popular among patients and clinicians [2].
Feldspathic ceramics, made from silica, are a commonly used ceramic material in aesthetic restorative dentistry as a part of inlays, onlays, and veneers. Ceramics require a durable bond to attach to the natural tooth structure. Adhesion between dental ceramics and resins is predicated on the physio-chemical interaction between the adhesive and ceramic [3]. This requires pre-conditioning of the ceramic surface for optimum bonding prior to cementation with a resin [4]. Conditioning and preparing the ceramic involves etching with hydrofluoric acid. The duration of etching and concentration of the acid can affect the final adhesive bond strength. The two main interfaces that bonding occurs at are the ceramic-cement interface and the adhesive-dentin interface [5]. Bond strength is determined by these two interfaces [6]. Clinical failures of ceramic restorations predominantly emanate from cemented surfaces [7,8,9]. The integrity of the conditioned surface and the resin affects treatment success and the longevity of the restoration [10,11]. Surface treatments of ceramics are a fundamental necessity for bonding and influence the appearance of the restoration and even microbial retention [12].
There are several techniques to precondition ceramic surfaces to enhance bond strength, including chemical, mechanical, and laser irradiation [4,10,13]. Hydrofluoric acid causes topographical changes including surface dissolutions, which allows for micromechanical retention [13]. Etching using hydrofluoric acid is a popular method for conditioning surfaces. However, it often requires an additional step of the application of a silane coupling agent for adequate strength [14,15]. Hydrofluoric acid is hazardous to soft tissues [16]. Exposure can lead to irreparable damage to the eyes, and risks, such as necrosis and bone decalcification, make it a precarious substance to handle and employ [17,18]. Such concerns necessitate the exploration of different etching protocols which provide reliable long-term bonding to ceramics as alternatives to hydrofluoric acid [19,20].
Mechanical methods of surface conditioning involve air abrasion using aluminum oxide particles or diamond burs to roughen the ceramic surface [21]. Roughening with burs at high speed produces a reliably retentive surface. Though diamond bur roughening in combination with other surface modification methods may yield better bond strength, they can cause a reduction in the strength of the restoration [22]. Burs have an added risk of crack formation, which may propagate over time, leading to the failure of a restoration [23,24].
Laser irradiation is a modern method of conditioning ceramic surfaces to ensure adhesion. Er:YAG, carbon dioxide (CO2), and Nd:YAG lasers can be used to condition the surfaces of ceramics prior to cementation. Lasers accumulate and focus an enormous amount of energy to a small circumscribed target area, which absorbs the energy and causes mircromorphological physical changes. The carbon dioxide laser (CO2) is commonly used intraorally in soft tissue and hard tissue applications [25,26]. Dental porcelain approximately absorbs CO2 laser wavelength. CO2 laser is very suitable for the surface treatment of ceramic materials [27]. CO2 laser etching may represent an effective method for conditioning zirconia surfaces, enhancing micromechanical retention, and improving the bond strength [28]. Conchoidal tears appear as a result of surface warming because of a heat initiation of ceramic surfaces by the focusing of the CO2 laser, which may lead to mechanical success between resin composite and ceramics retention [26,27,28,29,30]. Parameters of wavelength, frequency of laser, and output power dictate the characteristics of the irradiated surface [30,31]. CO2 lasers can produce sufficient bond strength in zirconia ceramics [32]. They have also been shown to increase surface roughness and wettability for certain CAD/CAM ceramics [33]. Lasers roughen the surface of feldspathic ceramic, enhancing micromechanical retention and improving the bond strength [30,31,32]. A few comparative studies have examined the laser treatment of feldspathic ceramic masses, leading to a lack of consensus on the best method to produce optimal bond strength in feldspathic ceramics [15,30,31,32,33,34,35,36,37,38].
Herein, we hypothesize that the conditioning treatments may influence the surface microstructure on ceramic and, thereby, have an impact on bond strength. On the other hand, characterization of the surface microstructure of the conditioned ceramic would augment our understanding of the influence of conditioning treatments. Considering the lack of clinical evidence for alternatives to hydrofluoric acid for conditioning ceramics, the present study evaluated the effect of three different surface conditioning techniques on the bonding between dual-cure resin luting cement and surface-treated feldspathic ceramic specifically focus surfaces assessment with scanning electron microscope, shear bond strength, and nature of bond failure.

2. Materials and Methods

2.1. Ceramic Disc Fabrication and Test Specimens Grouping

Feldspathic ceramic (CERAMCO 3 (Dentsply, Burlington, NJ, USA)), a mixture of potassium feldspar, and glass is in the feldspathic porcelains. After incongruent melting, feldspathic porcelains contain 19 weight percentage (wt%) of leucite crystals (K2O∙Al2O3∙4SiO2). Pre weighted (0.7 gm) low fusing feldspathic ceramic powder was mixed with 200 µL of modeling liquid to form a slurry. The slurry was packed in the custom-made metallic mold and gently tapped on a vibrator to ensure no voids were formed. Blotting paper was used to remove the excess water. The disc was then retrieved with gentle pressure and placed on a custom-made phosphate bonded slab for firing. Disc specimens were fired in a Touch & Press Furnace (Dentsply Sirona, Charlotte, NC, USA) according to manufacturers’ instructions. Initially, specimens were preheated for 5 min from 0 to 650 °C and then the temperature was maintained at 650 °C for another 5 min. The temperature was raised from 650 °C to 930 °C for 5 min at 50 hPa, followed by a vacuum hold for 1 min at 930 °C at 984 hPa. The vacuum was released to complete the firing cycle. Sixty ceramic test specimens with 4 mm thickness and 10 mm diameter were fabricated (Figure 1). These 60 samples of discs were divided into four groups:
  • Group A—Treated with 9.6% hydrofluoric acid
  • Group B—Treated with coarse diamond burs
  • Group C—Treated with CO2 laser
  • Group D—Control group without any surface treatment.

2.2. Treating the Surface of Test Specimens

Surface treatment was applied to the self-glazed surface of the prepared ceramic discs. The ceramic discs were placed and fixed in prefabricated plastic plates (dimension: 65 mm × 18 mm). Transparent adhesive tape (ScotchTM, 3M, St. Paul, MN, USA) was used to secure the self-glazed surface from contamination. The disc was then secured with self-cure acrylic resin (DPI-RR acrylic, Mumbai, India). The surfaces were standardized using abrasive papers, progressing from a rougher to smoother grit. First, 400 grit silicon carbide paper was used to smooth the surfaces, followed by 600 grit silicon carbide papers (3M, St. Paul, MN, USA) to gradually ground the specimen surface. This was followed by a ten-second polish on a 300 rpm grinding machine (Beuhler Metaserv, Leinfelden-Echterdingen, Germany) with a water coolant. All specimens were cleansed in the running water and dried. The dried specimens were etched for 1 min with 38% phosphoric acid to clean the abrasive particles followed by ultrasonic cleaning for 1 min and then air-dried. Subsequently, the specimens were randomly divided into four groups for the different surface treatment methods. Group A was treated with 9.6% hydrofluoric acid (Pulpdent, Watertown, MA, USA) for 5 min and 30 s, rinsed with water, and then dried for 30 s with an oil-free air syringe. Group B was treated with SF 11 coarse straight fissure diamond bur (Mani, Mumbai, India) with the help of a modified dental surveyor. Group C specimens underwent laser irradiation using a CO2 laser (Smart US20D, DEKA, Florence, Italy) running at a power of 13 W working at 10.6 µm in a continuous and non-contact mode. The applicator tip measured 1 mm in diameter with a length of 12 mm. The applicator tip was applied to the ceramic surfaces with a light contact for a period of 20 s in ‘super mode’. Group D served as the control group and, therefore, did not receive surface treatment.

2.3. Observation of the Treated Surfaces of the Specimen under SEM

Specimens were sputter-coated with a gold-palladium alloy (Bal-Tec SCD 050 Sputter Coater, Bal-Tec AG, Balzers, Liechtenstein) and examined under scanning electron microscopy (JSM-5500, Jeol Ltd., Tokyo, Japan) at 15 KV in backscattered mode to determine the surface changes on the ceramic discs after treatment. The treated area of each ceramic specimen was examined and the topographical contours were viewed and photographed at original magnification ×2000.

2.4. Luting Ceramic Disc Specimen with Dual-Cure Resin Luting Agent and Storage

All disc surfaces were primed with a silane coupling agent (Pulpdent, Watertown, MA, USA) for 60 s and then air-dried. Afterward, two liquids of bonding agent and activator, i.e., prime & bond NT and self-cure activator, in equal quantities were combined in a mixing tray, as per the manufacturer’s instruction, and applied on all of the ceramic discs. The specimens were light-cured for 10 s, according to the manufacturer’s instructions. An overhead projector (OHP) sheet with a hole measuring 4 mm was placed, matching the hole, at the center of the ceramic disc. The second plate was then positioned just above the first plate, taking care that the OHP sheet should not get displaced. Machine screws were then used to tighten and stabilize both the plates together. The purpose of the 4 mm hole in the OHP sheet was to standardize the bonding area to a diameter of 4 mm. The resin cement was mixed as per the manufacturer’s instructions and then applied through the 6 mm holes of the second plastic plate over the ceramic disc and light cured for 20 s from all directions. After one hour, machine screws were removed and all samples of various groups were placed in distilled water at 37 °C for 24 h in the incubator to simulate oral conditions [25,26].

2.5. The Shear Bond between Resin Cement and Ceramic Disc Evaluation

After 24 h in the incubator at 37 °C, all specimens were removed, rinsed, and then tested for shear bond strength (SBS) between prepared specimens of ceramic discs and resin cement on an Instron universal testing machine (Instron model 4467 tabletop load frame, 825 University Ave, Norwood, MA, USA). Tests were performed with a crosshead speed of 1 mm/min. The jaws of the Instron machine were moving in the opposite direction to test the shear bond strength between the ceramic disc specimen and resin cement. The jaws of the testing machine were continually moving in opposite directions until bond failure (debonding) took place. As soon as the bond was broken the machine automatically stopped moving and the force at bond failure in Newtons (N) was recorded for each specimen. The SBS, in megapascal (MPa), was then calculated using the formula: Force/surface area of the bracket.

2.6. Evaluation of Nature of Bond Failure under a Stereomicroscope

After shear bond testing of all specimens, the samples were evaluated to examine the nature of bond failure under a stereomicroscope (Wild M3B, Heerbrugg, Switzerland) at a magnification of ×12 to categorize as: (1) Cohesive, (2) Adhesive, and (3) Mixed bond failure.

2.7. Statistical Analysis

Data analysis was performed using SPSS v14.0 software (IBM Statistics, SPSS, Chicago, IL, USA). The basic characteristics of shear bond strength (SPS) was represented in average and standard deviation (Mean ± SD). Additionally, one-way analysis of variance (ANOVA) was performed to determine significant differences between the SBS based on the conditioning methods by implementing post hoc Tukey’s test. The statistical significance was determined at p ≤ 0.05.

3. Results

3.1. Scanning Electron Microscope Examination of Surfaces

Group A: the SEM view showed an increased irregular surface, as shown in Figure 1. The average area of irregular surface (4.83 ± 1.78 µm) acquired due to the etching effect of hydrofluoric acid on the ceramic surface was calculated using image J software (Version 1.53p 4) (Table 1).
Group B: the SEM view revealed an irregular surface is achieved by abrasion of the ceramic disc with diamond bur. The mean area (0.27 ± 0.1 µm) of irregular surface created with diamond bur was shown in Table 1. On physical observation, less irregular surface was noticed in Group B compared to Group A (Figure 2). Additionally, the irregular surface attributed by diamond treatment was significantly less when compared to hydrofluoric acid (Table 1).
Group C: the SEM view showed marginal change on the surface of the CO2 laser treatment compared to Group A and B. The noticed irregularities were superficial, as shown in Figure 3. Furthermore, the mean area of irregular surface created by the CO2 laser treatment was shown in Table 1.
Group D: the untreated group (control) showing few irregular surfaces may be due to phosphoric acid and porosity within the ceramic disc (Figure 4). However, the calculated mean area of irregular surface in Group D was the least compared to other analyzed groups (Table 1).

3.2. Shear Bond Strength

The mean shear bond strength exhibited by Group D (control group) was 8.09 ± 1.74 MPa, which was the lowest in comparison to other specimens. The highest value of mean shear bond strength load was recorded with hydrofluoric acid (Group A—21.40 ± 3.57 MPa). Diamond burs (Group B—15.17 ± 1.99 MPa) showed slightly lower values of mean shear load in comparison to Group A. However, diamond bur roughening showed greater bond strength than lasers (Group C—10.60 ± 1.86 MPa) (Table 2). The comparative analysis based on mean shear bond strength using ANOVA showed significant differences between groups (p < 0.05) (Table 3), except Group C vs. Group D.

3.3. Nature of Bond Failure

The nature of bond failure was observed under the stereomicroscope at 40× (Figure 5, Figure 6 and Figure 7). Three types of bond failure, such as cohesive, adhesive, and mixed, were assessed for each specimen and their results were reported in Table 4. Cohesive type failure was noticed in the Group A specimen, whereas, Group B mainly showed a mixed type of bond failure. Alternatively, Group C and D showed an adhesive type failure in most of the specimens.

4. Discussion

Ceramics require surface treatment for reliable bonding between the tooth and the restoration. Surface treatments are expected to modify the smooth surface by generating irregular microporosities that allow for the penetration of bonding agents for micromechanical retention. Hence, surface etching before cementation is considered as the most important step in ceramic restorations. Furthermore, the choice of surface treatment and luting agent has a potential impact on clinical success and longevity. In this study, we use three different surface treatment techniques to alter the surface characteristics of ceramics to investigate the bonding efficiency of luting agents for potential dental application. The surface characteristic after etching was assessed using SEM and the efficiency of resin bonding was determined by shear bond strength and nature bond failures. Appreciable changes in surface morphology were noted to significantly contribute to the bond strength based on the employed surface conditioning methods.
Three potential surface conditioning methods, such as (1) hydrofluoric acid, (2) diamond burs, and (3) CO2 laser, were adopted to generate rough surface on the ceramic and compared with the control (untreated ceramic) [39,40,41,42,43,44,45,46,47,48]. In light of the obtained results, treatment with the hydrofluoric acid, diamond burs, and CO2 laser showed significant change in the morphology of the ceramic surface compared to the control. Interestingly, the observed morphological changes with hydrofluoric acid treatment covers a wide area (4.83 ± 1.78 µm) of irregularity compared to the other two techniques, as determined from SEM image analysis using image J software. Whereas, the burs treatment showed moderate irregularity and the CO2 laser showed the least irregularity compared to the control. Notably, the surface micromorphology, in terms of pores and grooves pattern, width, and depth, was considerably enormous in the hydrofluoric acid treatment, which may critically support bonding the ceramics with resin composites. Interestingly, variable sizes of grooves and pores were observed in the specimens with the hydrofluoric acid treatment. This observation supports the results of previously published studies that described the hydrofluoric acid etching appearance as tunnel-like with a honey-comb-like microretentive pattern [39,40,41]. Furthermore, Posritong et al. and Sato et al. showed the formation of a microstructure on glass and lithium disilicate ceramics upon hydrofluoric acid etching that produce flexural strength to the cement [40,41]. Additionally, hydrofluoric acid helps to remove the glassy matrix selectively, exposing the crystalline structures and influencing the formation of microporosities [27]. Alternatively, there are few studies that demonstrate that increased surface roughness may not always lead to an increase in bond strength [28,29]. Hydrolysis and degradation of the adhesive hybrid layer may occur in cases of inadequate moisture control that lead to failure [30,31].
Shear bond strength was assessed after cementation using the Instron universal testing machine. The hydrofluoric acid based ceramic etching showed the greatest bond strength among the analyzed groups (Table 2). The surface roughening with the diamond burs and the CO2 laser group showed marginal shear bond strength compared to the untreated control group. The least bond strength was noticed in the untreated control, indicating that surface roughening on ceramics benefit efficient bonding [29,30,31]. This finding supports previous research in this area that shows hydrofluoric acid etching achieves greater effective bond strength compared to laser and mechanical conditioning [49,50,51]. Our findings are also in accord with previous studies by Shiu et al. and Akyil et al., which suggest that laser etching produces insufficient bond strength with feldspathic ceramic [7,47]. However, Hosseini et al. reported that surface treatment with lasers at a power of 1.5 to 2 W provided similar bond strengths as hydrofluoric acid etching [51]. In contrast to our findings, Barutcigil et al. examined the influence of different surface treatment methods on the shear bond strength of hybrid ceramic materials and found no difference between the techniques [52]. This disagreement might be due to the influence factors, such as acid concentration, application time, and specimen geometry.
In addition to the shear bond strength, this study evaluated the nature of bond failure acquired for the conditioning method upon cementation. Laser conditioned specimens showed an adhesive type of failure. This may be due to inadequate bonding between the resin and the ceramic surface because of a lack of roughness. It indicates that laser irradiation produces insufficient roughness for consistently reliable bond strength. The hydrofluoric acid group showed a cohesive type of failure. These results are in agreement with the findings of Moura et al. who noted hydrofluoric acid showed cohesive type failures with microshear testing [53]. This mode of failure may be related to the concentration of the acid used. Mokhtarpour et al. reported that reduced concentrations of hydrofluoric acid etchant could lead to cohesive types of failure [54]. In contrast to this, Neto et al. reported that lower concentrations of acid would result in poor bonding and lead to further adhesive failures [55]. Alternatively, increasing concentrations of hydrofluoric acid may result in loss of flexural strength. Etching time could also be an integral part of this equation with overetching ostensibly leading to non-homogeneous stress distribution during microshear bond testing.
Overall, our study revealed that the ceramic etching with hydrofluoric acid remains the most effective method, as evident from the SEM and bond strength analysis. Treating ceramic surfaces with 9.6% hydrofluoric acid produces a suitable surface for the resin bonding. However, hydrofluoric acid is caustic and hazardous to the patient and the clinician [56]. Careful and better clinical handling will be necessary to ensure that hydrofluoric acid is a gold standard that generates a rough surface on ceramic and supports micromechanical retention with resin composites. Although, this study is limited by its in vitro nature, which may not adequately simulate a true oral environment. Thus, findings of this study must be interpreted with caution when extrapolating to clinical settings with human subjects. Future studies should subject specimens to mechanical and thermal cycling to simulate the stresses and oral environment and examine the fractal geometry of various microstructures to assess the effects of various surface treatments.

5. Conclusions

In conclusion, our study demonstrates the effect of surface treatment with hydrofluoric acid prior to adhesive cementation that significantly contributes on shear bond strength with the resin cement compared to etching methods. Although the hydrofluoric acid was hazardous to health, careful handling may benefit the patient to achieve better ceramic restoration. Further, analyzing the effect of ceramics adhesion with different concentrations of hydrofluoric acid and relating the outcome with a benefit-risk assessment may open up new avenues in dental implantation.

Author Contributions

Conceptualization, S.G., M.H.D.A.W. and W.R.; methodology, B.G. and A.R.; software, B.K.M. and B.Z.; validation, S.B. (Sultan Binalrimal), V.P.V. and S.B. (Shilpa Bhandi); formal analysis, W.R. and B.K.M.; investigation, S.B. (Sultan Binalrimal) and B.G.; resources, A.T.R. and S.G.; data curation, B.Z. and S.P.; writing—original draft preparation, S.G., S.P., B.G., W.R., B.K.M. and M.H.D.A.W.; writing—review and editing, S.B. (Sultan Binalrimal), A.R., V.P.V., S.B. (Shilpa Bhandi), A.T.R. and B.Z.; visualization, A.T.R. and S.B. (Shilpa Bhandi); supervision, V.P.V. and A.R.; project administration, M.H.D.A.W. and S.P. All authors have read and agreed to the published version of the manuscript.

Funding

This research received no external funding.

Institutional Review Board Statement

Not applicable.

Informed Consent Statement

Not applicable.

Data Availability Statement

Not applicable.

Conflicts of Interest

The authors declare no conflict of interest.

References

  1. Contrepois, M.; Soenen, A.; Bartala, M.; Laviole, O. Marginal adaptation of ceramic crowns: A systematic review. J. Prosthet. Dent. 2013, 110, 447–454.e10. [Google Scholar] [CrossRef] [PubMed]
  2. Rosenstiel, S.; Land, M. Contemporary Fixed Prosthodontics-E-Book; Elsevier Health Sciences: Amsterdam, The Netherlands, 2015. [Google Scholar]
  3. Pisani-Proenca, J.; Erhardt, M.C.G.; Valandro, L.F.; Gutierrez-Aceves, G.; Bolanos-Carmona, M.V.; Del Castillo-Salmeron, R.; Bottino, M.A. Influence of ceramic surface conditioning and resin cements on microtensile bond strength to a glass ceramic. J. Prosthet. Dent. 2006, 96, 412–417. [Google Scholar] [CrossRef] [PubMed]
  4. Ozcan, M.; Vallittu, P.K. Effect of surface conditioning methods on the bond strength of luting cement to ceramics. Dent. Mater. 2003, 19, 725–731. [Google Scholar] [CrossRef] [Green Version]
  5. Graiff, L.; Piovan, C.; Vigolo, P.; Mason, P.N. Shear bond strength between feldspathic CAD/CAM ceramic and human dentine for two adhesive cements. J. Prosthodont. 2008, 17, 294–299. [Google Scholar] [CrossRef] [PubMed]
  6. Santos, G.C., Jr.; Santos, M.J.M.C.; Rizkalla, A.S. Adhesive Cementation of Etchable Ceramic Esthetic Restorations. J. Can. Dent. Assoc. 2009, 75, 379–384. [Google Scholar] [PubMed]
  7. Shiu, P.; De Souza-Zaroni, W.C.; Eduardo, C.D.P.; Youssef, M.N. Effect of feldspathic ceramic surface treatments on bond strength to resin cement. Photomed. Laser Surg. 2007, 25, 291–296. [Google Scholar] [CrossRef]
  8. May, L.G.; Kelly, J.R.; Bottino, M.A.; Hill, T. Influence of the resin cement thickness on the fatigue failure loads of CAD/CAM feldspathic crowns. Dent. Mater. 2015, 31, 895–900. [Google Scholar] [CrossRef] [Green Version]
  9. May, L.G.; Kelly, J.R.; Bottino, M.A.; Hill, T. Effects of cement thickness and bonding on the failure loads of CAD/CAM ceramic crowns: Multi-physics FEA modeling and monotonic testing. Dent. Mater. 2012, 28, e99–e109. [Google Scholar] [CrossRef]
  10. Matinlinna, J.P.; Vallittu, P.K. Bonding of resin composites to etchable ceramic surfaces–an insight review of the chemical aspects on surface conditioning. J. Oral Rehabil. 2007, 34, 622–630. [Google Scholar] [CrossRef]
  11. Campos, F.; Almeida, C.S.; Rippe, M.P.; De Melo, R.M.; Valandro, L.F.; Bottino, M.A. Resin bonding to a hybrid ceramic: Effects of surface treatments and aging. Oper. Dent. 2016, 41, 171–178. [Google Scholar] [CrossRef] [Green Version]
  12. Poole, S.F.; Pitondo-Silva, A.; Oliveira-Silva, M.; Moris, I.C.M.; Gomes, E.A. Influence of different ceramic materials and surface treatments on the adhesion of Prevotella intermedia. J. Mech. Behav. Biomed. Mater. 2020, 111, 104010. [Google Scholar] [CrossRef] [PubMed]
  13. Özcan, M.; Volpato, C.A. Surface conditioning protocol for the adhesion of resin-based materials to glassy matrix ceramics: How to condition and why. J. Adhes. Dent. 2015, 17, 292–293. [Google Scholar] [PubMed]
  14. Venturini, A.B.; Prochnow, C.; May, L.G.; Bottino, M.C.; Valandro, L.F. Influence of hydrofluoric acid concentration on the flexural strength of a feldspathic ceramic. J. Mech. Behav. Biomed. Mater. 2015, 48, 241–248. [Google Scholar] [CrossRef] [PubMed]
  15. Akova, T.; Yoldas, O.; Toroglu, M.S.; Uysal, H. Porcelain surface treatment by laser for bracket-porcelain bonding. Am. J. Orthod. Dentofac. Orthop. 2005, 128, 630–637. [Google Scholar] [CrossRef]
  16. Carvalho, R.; Martins, M.; De Queiroz, J.; Leite, F.P.P.; Özcan, M. Influence of silane heat treatment on bond strength of resin cement to a feldspathic ceramic. Dent. Mater. J. 2011, 30, 392–397. [Google Scholar] [CrossRef] [Green Version]
  17. Ramakrishnaiah, R.; Alkheraif, A.A.; Divakar, D.D.; Matinlinna, J.P.; Vallittu, P.K. The effect of hydrofluoric acid etching duration on the surface micromorphology, roughness, and wettability of dental ceramics. Int. J. Mol. Sci. 2016, 17, 822. [Google Scholar] [CrossRef] [Green Version]
  18. Carpena, G.; Ballarin, A. Hydrofluoric Acid—Simple Things You May Do Not Know about Something You Are So Habituated to Use. Odovtos-Int. J. Dent. Sci. 2015, 1, 15–23. [Google Scholar] [CrossRef] [Green Version]
  19. Dennerlein, K.; Kiesewetter, F.; Kilo, S.; Jäger, T.; Göen, T.; Korinth, G.; Drexler, H. Dermal absorption and skin damage following hydrofluoric acid exposure in an ex vivo human skin model. Toxicol. Lett. 2016, 248, 25–33. [Google Scholar] [CrossRef]
  20. Al Edris, A.; Al Jabr, A.; Cooley, R.L.; Barghi, N. SEM evaluation of etch patterns by three etchants on three porcelains. J. Prosthet. Dent. 1990, 64, 734–739. [Google Scholar] [CrossRef]
  21. Guruprasada; Rivankar, N.; Dhiman, R.K.; Viswambaran, M. Evaluation of the effect of surface preparation using phosphoric acid and luting cement on the flexural strength of porcelain laminate veneering material. Med. J. Armed Forces India 2015, 71, S299–S305. [Google Scholar] [CrossRef] [Green Version]
  22. Kupiec, K.A.; Wuertz, K.M.; Barkmeier, W.W.; Wilwerding, T.M. Evaluation of porcelain surface treatments and agents for composite-to-porcelain repair. J. Prosthet. Dent. 1996, 76, 119–124. [Google Scholar] [CrossRef]
  23. Bessing, C.; Wiktorsson, A. Comparison of two different methods of polishing porcelain. Scand. J. Dent. Res. 1983, 91, 482–487. [Google Scholar] [CrossRef] [PubMed]
  24. Peterson, I.M.; Pajares, A.; Lawn, B.R.; Thompson, V.P.; Rekow, E.D. Mechanical characterization of dental ceramics by hertzian contacts. J. Dent. Res. 1998, 77, 589–602. [Google Scholar] [CrossRef] [PubMed]
  25. Hatanaka, G.R.; Polli, G.S.; Fais, L.M.G.; Reis, J.M.D.S.N.; Pinelli, L.A.P. Zirconia changes after grinding and regeneration firing. J. Prosthet. Dent. 2017, 118, 61–68. [Google Scholar] [CrossRef] [PubMed] [Green Version]
  26. Pick, R.M.; Colvard, M.D. Current status of lasers in soft tissue dental surgery. J. Periodontol. 1993, 64, 589–602. [Google Scholar] [CrossRef] [PubMed]
  27. Ural, Ç.; Külünk, T.; Külünk, S.; Kurt, M. The effect of laser treatment on bonding between zirconia ceramic surface and resin cement. Acta Odontol. Scand. 2010, 68, 354–359. [Google Scholar] [CrossRef]
  28. Akyil, M.S.; Uzun, I.H.; Bayindir, F. Bond strength of resin cement to yttrium-stabilized tetragonal zirconia ceramic treated with air abrasion, silica coating, and laser irradiation. Photomed. Laser Surg. 2010, 28, 801–808. [Google Scholar] [CrossRef]
  29. Ersu, B.; Yuzugullu, B.; Yazici, A.R.; Canay, S. Surface roughness and bond strengths of glass-infiltrated alumina ceramics prepared using various surface treatments. J. Dent. 2009, 37, 848–856. [Google Scholar] [CrossRef]
  30. Chen, J.R.; Oka, K.; Kawano, T.; Goto, T.; Ichikawa, T. Carbon dioxide laser application enhances the effect of silane primer on the shear bond strength between porcelain and composite resin. Dent. Mater. J. 2010, 29, 731–737. [Google Scholar] [CrossRef] [Green Version]
  31. Dilber, E.; Yavuz, T.; Kara, H.B.; Ozturk, A.N. Comparison of the effects of surface treatments on roughness of two ceramic systems. Photomed. Laser Surg. 2012, 30, 308–314. [Google Scholar] [CrossRef]
  32. Stübinger, S.; Homann, F.; Etter, C.; Miskiewicz, M.; Wieland, M.; Sader, R. Effect of Er: YAG, CO2 and diode laser irradiation on surface properties of zirconia endosseous dental implants. Lasers Surg. Med. 2008, 40, 223–228. [Google Scholar] [CrossRef] [PubMed]
  33. El Gamal, A.; Medioni, E.; Rocca, J.P.; Fornaini, C.; Muhammad, O.H.; Brulat-Bouchard, N. Shear bond, wettability and AFM evaluations on CO2 laser-irradiated CAD/CAM ceramic surfaces. Lasers Med. Sci. 2017, 32, 779–785. [Google Scholar] [CrossRef] [PubMed]
  34. Yucel, M.T.; Aykent, F.; Akman, S.; Yondem, I. Effect of surface treatment methods on the shear bond strength between resin cement and all-ceramic core materials. J. Non-Cryst. Solids 2012, 358, 925–930. [Google Scholar] [CrossRef]
  35. Malysa, A.; Wezgowiec, J.; Orzeszek, S.; Florjanski, W.; Zietek, M.; Wieckiewicz, M. Effect of Different Surface Treatment Methods on Bond Strength of Dental Ceramics to Dental Hard Tissues: A Systematic Review. Molecules 2021, 26, 1223. [Google Scholar] [CrossRef] [PubMed]
  36. Geramipanah, F.; Majidpour, M.; Sadighpour, L.; Fard, M.J.K. Effect of artificial saliva and pH on shear bond strength of resin cements to zirconia-based ceramic. Eur. J. Prosthodont. Restor. Dent. 2013, 21, 5–8. [Google Scholar]
  37. Ayad, M.F.; Fahmy, N.Z.; Rosenstiel, S.F. Effect of surface treatment on roughness and bond strength of a heat-pressed ceramic. J. Prosthet. Dent. 2008, 99, 123–130. [Google Scholar] [CrossRef]
  38. Borges, G.A.; Sophr, A.M.; de Goes, M.F.; Sobrinho, L.C.; Chan, D.C.N. Effect of etching and airborne particle abrasion on the microstructure of different dental ceramics. J. Prosthet. Dent. 2003, 89, 479–488. [Google Scholar] [CrossRef]
  39. Bottino, M.C.; Özcan, M.; Coelho, P.G.; Valandro, L.F.; Bressiani, J.C.; Bressiani, A.H.A. Micro-morphological changes prior to adhesive bonding: High-Alumina and glassy-matrix ceramics. Braz. Oral Res. 2008, 22, 158–163. [Google Scholar] [CrossRef] [Green Version]
  40. Posritong, S.; Borges, A.L.S.; Chu, T.G.; Eckert, G.J.; Bottino, M.A.; Bottino, M.C. The impact of hydrofluoric acid etching followed by unfilled resin on the biaxial strength of a glass-ceramic. Dent. Mater. 2013, 29, e281–e290. [Google Scholar] [CrossRef]
  41. Prado Sato, T.; Cotes, C.; Yamamoto, L.T.; Rossi, N.R.; Macedo, V.C.; Kimpara, E.T. Flexural strength of a pressable lithium disilicate ceramic: Influence of surface treatments. Appl. Adhes. Sci. 2013, 1, 7. [Google Scholar] [CrossRef] [Green Version]
  42. Kara, H.B.; Ozturk, A.N.; Aykent, F.; Koc, O.; Ozturk, B. The effect of different surface treatments on roughness and bond strength in low fusing ceramics. Lasers Med. Sci. 2011, 26, 599–604. [Google Scholar] [CrossRef] [PubMed]
  43. Kern, M.; Barloi, A.; Yang, B. Surface conditioning influences zirconia ceramic bonding. J. Dent. Res. 2009, 88, 817–822. [Google Scholar] [CrossRef] [PubMed]
  44. Amin Salehi, E.; Heshmat, H.; Moravej Salehi, E.; Javad Kharazifard, M. In Vitro Evaluation of the Effect of Different Sandblasting Times on the Bond Strength of Feldspathic Porcelain to Composite Resin. JIDA 2013, 25, 68–75. [Google Scholar]
  45. Escribano, N.; de la Macorra, J.C. Microtensile bond strength of self-adhesive luting cements to ceramic. J. Adhes. Dent. 2006, 8, 337. [Google Scholar]
  46. Guarda, G.B.; Gonçalves, L.S.; Correr, A.B.; Moraes, R.R.; Sinhoreti, M.A.C.; Correr-Sobrinho, L. Luting glass ceramic restorations using a self-adhesive resin cement under different dentin conditions. J. Appl. Oral Sci. 2010, 18, 244–248. [Google Scholar] [CrossRef] [PubMed] [Green Version]
  47. Akyil, M.S.; Yilmaz, A.; Bayindir, F.; Duymus, Z.Y. Microtensile bond strength of resin cement to a feldspathic ceramic. Photomed. Laser Surg. 2011, 29, 197–203. [Google Scholar] [CrossRef]
  48. Hayakawa, T.; Horie, K.; Aida, M.; Kanaya, H.; Kobayashi, T.; Murata, Y. The influence of surface conditions and silane agents on the bond of resin to dental porcelain. Dent. Mater. 1992, 8, 238–240. [Google Scholar] [CrossRef]
  49. Kursoglu, P.; Motro, P.F.K.; Yurdaguven, H. Shear bond strength of resin cement to an acid etched and a laser irradiated ceramic surface. J. Adv. Prosthodont. 2013, 5, 98–103. [Google Scholar] [CrossRef] [Green Version]
  50. Yavuz, T.; Dilber, E.; Kara, H.B.; Tuncdemir, A.R.; Ozturk, A.N. Effects of different surface treatments on shear bond strength in two different ceramic systems. Lasers Med. Sci. 2013, 28, 1233–1239. [Google Scholar] [CrossRef]
  51. Hosseini, M.H.; Sobouti, F.; Etemadi, A.; Chiniforush, N.; Shariati, M. Shear bond strength of metal brackets to feldspathic porcelain treated by Nd:YAG laser and hydrofluoric acid. Lasers Med. Sci. 2015, 30, 837–841. [Google Scholar] [CrossRef]
  52. Barutcigil, K.; Barutcigil, Ç.; Kul, E.; Özarslan, M.M.; Buyukkaplan, U.S. Effect of Different Surface Treatments on Bond Strength of Resin Cement to a CAD/CAM Restorative Material. J. Prosthodont. 2019, 28, 71–78. [Google Scholar] [CrossRef] [PubMed]
  53. Moura, D.M.D.; de Araújo, A.M.M.; de Souza, K.B.; Veríssimo, A.H.; Tribst, J.P.M.; de Assunção e Souza, R.O. Hydrofluoric acid concentration, time and use of phosphoric acid on the bond strength of feldspathic ceramics. Braz. Oral Res. 2020, 34, 1–10. [Google Scholar] [CrossRef] [PubMed]
  54. Mokhtarpour, F.; Alaghehmand, H.; Khafri, S. Effect of hydrofluoric acid surface treatments on micro-shear bond strength of CAD/CAM ceramics. Electron. Physician 2017, 9, 5487–5493. [Google Scholar] [CrossRef] [PubMed] [Green Version]
  55. Sundfeld Neto, D.; Naves, L.Z.; Costa, A.R.; Correr, A.B.; Consani, S.; Borges, G.A.; Correr-Sobrinho, L. The effect of hydrofluoric acid concentration on the bond strength and morphology of the surface and interface of glass ceramics to a resin cement. Oper. Dent. 2015, 40, 470–479. [Google Scholar] [CrossRef] [Green Version]
  56. Özcan, M.; Allahbeickaraghi, A.; Dündar, M. Possible hazardous effects of hydrofluoric acid and recommendations for treatment approach: A review. Clin. Oral Investig. 2012, 16, 15–23. [Google Scholar] [CrossRef]
Figure 1. Group A: etching effect of hydrofluoric acid on the ceramic surface at ×2000 under SEM.
Figure 1. Group A: etching effect of hydrofluoric acid on the ceramic surface at ×2000 under SEM.
Coatings 12 00399 g001
Figure 2. Group B: surface treatment of diamond bur on the ceramic surface at ×2000 under SEM.
Figure 2. Group B: surface treatment of diamond bur on the ceramic surface at ×2000 under SEM.
Coatings 12 00399 g002
Figure 3. Group C: surface treatment of the CO2 laser on the ceramic surface at ×2000 under SEM.
Figure 3. Group C: surface treatment of the CO2 laser on the ceramic surface at ×2000 under SEM.
Coatings 12 00399 g003
Figure 4. Control group (Group D): without surface treatment on the ceramic surface at ×2000 under SEM.
Figure 4. Control group (Group D): without surface treatment on the ceramic surface at ×2000 under SEM.
Coatings 12 00399 g004
Figure 5. The specimen shows a cohesive type of bond failure.
Figure 5. The specimen shows a cohesive type of bond failure.
Coatings 12 00399 g005
Figure 6. The specimen shows a mixed type of bond failure.
Figure 6. The specimen shows a mixed type of bond failure.
Coatings 12 00399 g006
Figure 7. The specimen shows an adhesive type of bond failure.
Figure 7. The specimen shows an adhesive type of bond failure.
Coatings 12 00399 g007
Table 1. Average irregular surface acquired after etching with hydrofluoric acid, diamond burs, and CO2 laser, and control group.
Table 1. Average irregular surface acquired after etching with hydrofluoric acid, diamond burs, and CO2 laser, and control group.
AreaGroup AGroup BGroup CGroup D
Mean (µm)4.8380.2760.20.15
SD1.780.10.0940.045
Table 2. Characteristics of mean shear bond strength acquired due to hydrofluoric acid, diamond burs, and CO2 laser treatment, and control.
Table 2. Characteristics of mean shear bond strength acquired due to hydrofluoric acid, diamond burs, and CO2 laser treatment, and control.
GroupNMeanStd. Dev.95% Confidence Interval for Mean
Lower BoundUpper Bound
Group A1521.403.5719.4223.38
Group B1515.171.9914.0616.27
Group C1510.601.869.5611.63
Group D158.091.747.139.06
Table 3. Comparison of mean shear bond strength between the treatment and control group.
Table 3. Comparison of mean shear bond strength between the treatment and control group.
GroupSample SizeStatistical Significance
Group AGroup BGroup CGroup D
Group A151p ≤ 0.001p ≤ 0.001p ≤ 0.001
Group B15p ≤ 0.0011p ≤ 0.001p ≤ 0.001
Group C15p ≤ 0.001p ≤ 0.0011p = 0.52572
Group D15p ≤ 0.001p ≤ 0.001p = 0.525721
p-value ≤ 0.05, statistically significant.
Table 4. Type of bond failure between the analyzed groups.
Table 4. Type of bond failure between the analyzed groups.
Nature of Bond FailureGroup AGroup BGroup CGroup D
Cohesive15030000
Mixed00120100
Adhesive00001415
Publisher’s Note: MDPI stays neutral with regard to jurisdictional claims in published maps and institutional affiliations.

Share and Cite

MDPI and ACS Style

Gupta, S.; Gupta, B.; Motwani, B.K.; Binalrimal, S.; Radwan, W.; Robaian, A.; Zidane, B.; Al Wadei, M.H.D.; Veeraraghavan, V.P.; Bhandi, S.; et al. The Effect of Different Surface Conditioning Techniques on the Bonding between Resin Cement & Ceramic. Coatings 2022, 12, 399. https://doi.org/10.3390/coatings12030399

AMA Style

Gupta S, Gupta B, Motwani BK, Binalrimal S, Radwan W, Robaian A, Zidane B, Al Wadei MHD, Veeraraghavan VP, Bhandi S, et al. The Effect of Different Surface Conditioning Techniques on the Bonding between Resin Cement & Ceramic. Coatings. 2022; 12(3):399. https://doi.org/10.3390/coatings12030399

Chicago/Turabian Style

Gupta, Shekhar, Bharti Gupta, Bhagwandas K. Motwani, Sultan Binalrimal, Waseem Radwan, Ali Robaian, Bassam Zidane, Mohammed Hussain Dafer Al Wadei, Vishnu Priya Veeraraghavan, Shilpa Bhandi, and et al. 2022. "The Effect of Different Surface Conditioning Techniques on the Bonding between Resin Cement & Ceramic" Coatings 12, no. 3: 399. https://doi.org/10.3390/coatings12030399

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.

Article Metrics

Back to TopTop