Next Article in Journal
Gas-Solid Reaction Route toward the Production of Intermetallics from Their Corresponding Oxide Mixtures
Next Article in Special Issue
Nanocrystalline β-Ta Coating Enhances the Longevity and Bioactivity of Medical Titanium Alloys
Previous Article in Journal
Impurity Antimony-Induced Creep Property Deterioration and Its Suppression by Rare Earth Ceriumfor a 9Cr-1Mo Ferritic Heat-Resistant Steel
Previous Article in Special Issue
The Development of Coronary Artery Stents: From Bare-Metal to Bio-Resorbable Types
 
 
Font Type:
Arial Georgia Verdana
Font Size:
Aa Aa Aa
Line Spacing:
Column Width:
Background:
Article

Evaluation of Chill Cast Co-Cr Alloys for Biomedical Applications

by
Ana Laura Ramirez-Ledesma
1,
Hugo F. Lopez
2,* and
Julio Alberto Juarez-Islas
1
1
Instituto de Investigaciones en Materiales, Universidad Nacional Autonoma de Mexico, Av. Universidad 3000, Circuito Exterior S/N, Cd. Universitaria, Mexico D.F. 04510, Mexico
2
Materials Science and Engineering Department, CEAS University of Wisconsin-Milwaukee, 3200 N. Cramer Street, Milwaukee, WI 53211, USA
*
Author to whom correspondence should be addressed.
Metals 2016, 6(8), 188; https://doi.org/10.3390/met6080188
Submission received: 15 April 2016 / Revised: 3 August 2016 / Accepted: 11 August 2016 / Published: 16 August 2016
(This article belongs to the Special Issue Metallic Biomaterials)

Abstract

:
Binary Co-Cr alloys containing various Cr contents were vacuum induction melted and cast into wedge-shaped copper molds. It was intended to develop a microstructure (1) free from interdendritic segregation and porosity; (2) having minimal intermetallic precipitates; and (3) suitable for biomedical applications. The resultant microstructures were evaluated from sections obtained longitudinally and centrally in the plane normal to the diverging wedge faces. All ingots showed a dendritic microstructure with some characteristic features. For instance, in Co-20–30 wt. % Cr alloys, the chilled cast microstructures consisted of columnar dendrites without interdendritic segregation, a minimum of intermetallic precipitates, and the presence of a predominantly athermal HCP ε-martensite (>80 vol. %). In addition, the metastable FCC γ-Co phase was identified by X-ray diffraction and scanning electron microscopy. In the case of 35–44 wt. % Cr cobalt alloys, a eutectic constituent including the σ-phase were found to develop in the interdendritic regions. From this work, a Co-20 wt. % Cr alloy was chosen for further investigation after heat treating below the γ/ε transition temperature. The resultant tensile strength and ductility were further improved after applying a heat treatment at 730 °C for 30 min, obtaining values of elongation of 26% as compared with 2.55 < 5 of elongation in the as cast condition. Also, the alloy corrosion resistance in artificial saliva was investigated. It was found that the exhibited corrosion rates for the as-cast and heat-treated conditions are between those reported for other similar systems.

Graphical Abstract

1. Introduction

Wrought and investment casting Co-Cr-Mo alloys have been widely employed for implant devices replacing hard tissue or in dental restorations in the human body [1,2]. These alloys are known to possess excellent biocompatibility, mechanical properties, as well as wear and corrosion resistance [3,4,5]. In as-cast cobalt alloys the solidified microstructures consist of a predominantly FCC γ-dendritic structure which is accompanied by segregation, and second phase precipitates within the matrix and along the interdendritic regions. In addition, inherent investment casting defects are of concern as they can lead to early implant failure and inadequate mechanical properties [6].
In general, investment casting Co-Cr-Mo alloys used as biomedical devices exhibit poor ductility, shrinkage porosity, interdendritic segregation, and the presence of intermetallic compounds [7,8]. Hence, in order to improve alloy performance for potential biomedical applications, modifications in alloy design and casting technology have been considered in order to enhance the strength and ductility of Co-based alloys [9]. In particular, changes in alloy design have been aimed at suppressing brittle-phase formation along the interdendritic regions during solidification.
As Co-Cr-Mo devices are expected to experience increasing use in a growing population of young patients, alloy reliability and safety levels become a major concern. Thus, further improvements in the exhibited mechanical properties of Co-alloys are desirable. One of the ways to achieve this goal has been through microstructural control, such as thermomechanical processing or heat-treating [10,11,12,13,14]. In addition, alternatives in alloy design to produce biocompatible-grade Ni-free alloys have been under investigation due to the inherent risks associated with Ni-related allergic responses [15,16].
From the published literature, it is apparent that in order to design a sound Co-based alloy for biomedical applications, the choice of alloying elements, processing conditions and resultant properties need to be clearly identified. In particular, it is desirable to attain optimal alloy strength and ductility, combined with a high corrosion resistance [17]. Accordingly, in this work, a novel approach is proposed that leads to optimum casting processing conditions which result in desirable mechanical properties, including corrosion resistance. The investigated alloys were as-cast segregation-free Co-Cr alloys intended for novel biomedical applications. For this purpose, wedge-shaped copper molds were employed in order to vary the cooling rates undergone by the as-cast alloys. The resultant alloy microstructures were subsequently characterized and out of these, the Co-20 wt. % Cr alloy was chosen for further characterization as they did not exhibit interdendritic segregation and the amount of precipitate was minimal. Moreover, in this alloy the effect of implementing a heat treatment below the γ/ε transition temperature on the mechanical properties and corrosion resistance was evaluated and compared with the as-cast condition

2. Materials and Methods

2.1. Materials Preparation

Cobalt alloys containing 20, 30, 35, 40, and 44 wt. % Cr were melted from pure Co (99.99%) and pure Cr (99.99%) in an alumina crucible using a vacuum induction furnace. Mo was not added because one aim of this work was to achieve a nearly free segregation microstructure with a minimum quantity of precipitates and carbides. The system was evacuated three times with high purity argon prior to vacuum melting. Once the alloy reached 2273 K (approx. 2000 °C), both Co and Cr were in liquid state and the chamber was immediately evacuated again to remove any gases dissolved in the liquid bath. At the same time, the temperature was dropped down to 1873 K (approx. 1600 °C) and a slag was formed in the bath surface. Afterwards, the liquid alloy was cast into a wedge-shaped copper mold. The wedge mold sides were covered by an alumina sheet to keep the heat flow predominantly in one direction, (see Figure 1). Prior to casting, Pt/Pt-18% Rh thermocouples were centrally inserted into the wedge copper mold at 20, 60, and 90 mm from the tip to the top of the mold cavity, at half thickness locations of 1.0, 3.0, and 4.5 mm, respectively. The as-cast ingots were then longitudinally and centrally sectioned in the plane normal to the diverging wedge faces and mechanically polished and electrolitically etched using a 60 vol. % HNO3 + 40 vol. % H2O solution and 6 volts.

2.2. Materials Characterization

The resultant microstructures were identified and characterized using a JEOL 7600 scanning electron microscope (SEM, Jeol, Tokyo, Japan) and a JEOL1200 EX, transmission electron microscope (TEM, Jeol, Tokyo, Japan coupled with energy dispersed X-ray microanalysis (EDS, Jeol, Tokyo, Japan). X-ray diffraction was carried out using a Siemens D-5000 diffractometer with a Kα-Cu (1.5418 Å, Siemens, Munich, Germany) radiation and a scanning angle, 2θ from 40° to 96° at a scanning rate of 1 °/min. Ingot sections of an alloy containing 20 wt. % Cr whose microstructures were dendritic, but segregation suppressed, were selected for heat treating. The implemented heat treatment was carried out at 1003.15 K (730 °C) for 60 min under an argon atmosphere [18]. This was followed by determinations of mechanical properties in a tensile testing machine, Instron 1210 (MTS Systems Corporation, Eden Prairie, MN, USA), at a strain rate ε ˙ = 1.6 × 10−4·s−1 and a travel speed of 0.5 mm/min.

2.3. Electrochemical Techniques

Preliminary corrosion tests were carried out using potentiodynamic polarization in a Gill AC potentiostat. For this purpose, the applied potential was varied from −1250 mV—with respect to the free corrosion potential, Ecorr—up to 1250 mV at a scanning rate of 0.5 mV/s. A conventional three-electrode glass cell was used with graphite as an auxiliary electrode and a saturated calomel electrode (SCE) as the reference. Corrosion current density values, Icorr, were estimated using the Tafel extrapolation method and by considering an extrapolation interval of ±250 mV around the Ecorr value, once stable. The electrolyte employed consisted of artificial saliva whose composition is given in Table 1.

3. Results

3.1. Cooling Rates and Microstructure

Figure 2a shows cooling curves at various locations of the wedge-shaped mold in the temperature range of 1873.15–1673.15 K (1600–1400 °C). Notice that the exhibited cooling rates are closely related to the thermocouple locations. In particular, it can be observed that the cooling rate for the Co-20 wt. % Cr alloy was 450 K/s at 20 mm from the tip (curve 1); 230 K/s at 60 mm, center (curve 2); and 120 K/s at 90 mm, top (curve 3). In addition, the location of the various solidified microstructures—including a eutectic and other intermetallic phases in the chilled-cast wedges for the various Cr contents (20, 30, 35, 40, and 44 wt. % Cr)—is shown in Figure 2b. Three dominant microstructures were identified: (1) dendrites; (2) dendrites and a eutectic in the interdendritic region; and (3) dendrites plus a eutectic and the σ-phase in the interdendritic region; this in agreement with other investigations [19].
Figure 3 shows the various microstructures found in the Co–Cr alloys located at 20, 60, and 90 mm from the tip to the top of the wedge, respectively. Notice that the dominant solidified microstructures are made up of columnar dendrites. The presence of interdendrite segregation was not detected for Cr contents ≤30 wt. %, indicating that interdendritic segregation and brittle phase formation can be suppressed through rapid solidification.
Figure 4 shows the dimensions of the interdendritic segregation regions in as-cast Co-alloys processed by the investment casting technique [2,7,20,21,22,23,24]. Notice that interdendritic segregation regions are on the order of 5–18 μm, but in atomized powders the interdendritic segregation diminishes down to close to 0.3 μm [25].
In the present work, interdendritic spaces below 0.25 μm were observed in the bulk microstructure. In addition, randomly distributed precipitates within the matrix and at interdendritic arms were identified by SEM microanalysis. Accordingly, the Co3Cr and CoCr intermetallic phases were found to precipitate with a volume fraction which varied from 2.4 × 10−3 (20 wt. % Cr) to 2.8 × 10−3 (30 wt. % Cr). Beyond this Cr content, copious precipitation of Co3Cr and CoCr occurred, so it was no longer possible to make accurate volume fraction determinations (see Figure 3d,e). Moreover, from the X-ray diffraction determinations (see Figure 5), it was found that dendrites were composed of athermal HCP ε-Co phase and metastable FCC γ-Co phase, and both phases were found to form in all the rapidly solidified alloys regardless of the Cr content. The amounts of athermal HCP ε-phase were determined by employing the expression proposed by Sage and Guillaud [26]:
HCP (vol. %) = I(l0Īl)HCP/ /I(l0Īl)HCP + 1.5 I(200)FCC
where I(200)FCC and I(l0Īl)HCP are the integrated intensities of the (200)γ and (l0Īl)ε diffraction peaks for the FCC and HCP phases, respectively.
Accordingly, using the exhibited intensity peaks, the amounts of athermal ε-martensite were estimated as a function of the applied cooling rates and Cr contents, and they are given in Table 2.
From this table, it is evident that in segregation-free alloys, the volume fractions of precipitated ε-phase where were 89.6% and 90.1% for 20% Cr and 30% Cr alloys, respectively. These results are given in Figure 6, where the vol. % ε-martensite is plotted as a function of alloy processing. In this regard, the percent of ε-Co phase in investment casting alloys exhibits a value between 2 and 12 vol. % [25,27], while in hot Co-alloy forgings (10% deformation) the amount of ε-phase reached a value of 35 vol. % [10]. Additionally, in atomized particles and chilled cast alloys (present work), 64 vol. % and 89.6–90.1 vol. % ε-phase were precipitated, respectively (Figure 6).
Figure 7 is an SEM micrograph of the athermal ε-martensite developed within the columnar dendritic structure in a Co-20 wt. % Cr alloy; in particular, notice the typical striations associated with the athermal ε-martensite transformation [28]. The exhibited microstructure was further investigated by TEM means.
Figure 8a is a TEM micrograph with its corresponding diffraction pattern (Figure 8b) showing a fine distribution of elongated athermal ε-plates within the columnar dendritic structure.

3.2. Mechanical and Corrosion Properties

Figure 9 shows stress-strain plots corresponding to the Co-20 wt. % Cr alloy in both the as-cast and heat-treated conditions. Notice from this figure that the alloy in the as-cast condition exhibits yield and ultimate tensile strengths of 230 MPa and 361 MPa, respectively, but an elongation of only 2.55%. Yet, after isothermal alloy heat treating at 1003.15 K for 60 min the mechanical properties exhibit a dramatic improvement in alloy strength of over 40% (i.e., 346 MPa yield strength and a UTS of 597 MPa).
An examination of the fracture surfaces (see Figure 10a) indicates that the as-cast alloy fractured in a somewhat brittle fashion along columnar interdendritic interfaces. Also, the fracture path shows ε-Co phase striations delineating the columnar dendrites. In contrast, the heat-treated alloy exhibited a highly ductile fracture mode which was accompanied by significant plastic deformation (up to 26% elongation) and dimple development (Figure 10b).
Finally, preliminary testing on the corrosion resistance of the Co-20 wt. % Cr alloy by potentiodynamic polarization in synthetic saliva was used for determinations of corrosion rates. Figure 11 and Table 3 show the corrosion potential, current density, and corrosion rate values found for the Co-20 wt. % Cr alloy in both, the as-cast, and after heat treating conditions. Notice that corrosion rates of 8 × 10−4 and 3.56 × 10−3 mm/year were found for the as-cast and treated alloys, respectively.

4. Discussion

4.1. Phases

Figure 12 shows a map of the various phases found as a function of the applied cooling rates and Cr contents where the presence of FCC γ-Co phase/HCP ε-Co phase is observed even for eutectic compositions. In the case of investment casting Co-Cr alloys, a highly inhomogeneous structure is expected to form with large-grained cored dendrites and Co-rich regions. In particular, the interdendritic regions can contain various quaternary Co-rich, Cr-rich, and Cr- and Mo-rich phases [30]. The microstructures found in the rapidly solidified Co-35 wt. % Cr, Co-40 wt. % Cr and Co-44 wt. % Cr alloys are in agreement with the ones reported by other workers [21,31,32], but for the binary Co-Cr system.
From this work, it is evident that rapid solidification either reduces or inhibits segregation at Cr contents below 30 wt. % (see Figure 13). Nevertheless, as the Cr-content increases, the columnar dendritic structure becomes heavily segregated at the interdendritic locations. X-ray diffraction determinations confirmed the presence of the eutectic constituent and of the σ-phase for chromium contents >30 wt. % (see Figure 5c,d). In addition, X-ray intensity peaks corresponding to the FCC γ-Co phase and HCP ε-Co phase were identified. Moreover, as the Cr content increases in the as-cast alloys, a reduction in the primary dendrite arm spacing was observed (see Figure 3). This effect is concomitant with an increase in interdendritic segregation (Co-40 and 44 wt. % Cr alloys) and with the precipitation of both, the eutectic and the σ-phase in agreement with other reports [21]. In contrast, in conventionally solidified as-cast microstructures the interdendritic regions are rather wide with spacings oscillating between 7 μm and 18 μm [7,31,32,33], as shown in Figure 4.

4.2. HCP and FCC Phases

In this work, it was found that the HCP ε-Co phase was able to form in all the rapidly solidified alloys regardless of the Cr content. According to the published literature [34], it is well-known that the athermal HCP ε-Co phase occurs by a martensitic transformation from the high temperature stable FCC γ-Co phase. The development of athermal ε-martensite is expected to be favored by rapid cooling from the γ-Co phase [34]. Nevertheless, in conventionally investment solidified Co-Cr-Mo-C alloys the reported amounts of precipitated ε-martensite have been found to be relatively small, not exceeding 20 vol. %, in most cases [35,36]. A maximum of 64 vol. % was reported in 80 μm water atomized Co-Cr-Mo powders (Figure 6) [25]. The amounts of athermal ε-martensite are strongly influenced by the annealing temperatures, with increasing volume fractions found in alloys annealed at increasing temperatures [34]. In contrast, under the cooling conditions achieved during chill casting of Co-Cr alloys, the amounts of precipitated athermal ε-martensite exceeded 80 vol. % as seen in Table 2.
SEM and TEM observations of the exhibited microstructures (see Figure 7 and Figure 8) are consistent with the ones reported by Rajan [37] for HCP martensite. From the electron diffraction pattern, it is found that the FCC γ-Co possesses a [11] zone axes, and a [01Ī0] one for the HCP ε-Co. In addition, these phases possess a (1Ī1)||(0002) orientation relationship. From Figure 8a it is evident that the FCC γ-Co phase is located between fine HCP ε-martensite plates. Apparently, a high density of ε-martensite plates nucleated and grew at expenses of the austenitic matrix, leaving residual γ-Co phase films in-between ε-martensite plates. Thus, copious nucleation of athermal ε-martensite seems to be strongly favored by the rapid cooling effects imposed on these alloys. According to Jones [38], it is expected that rapid solidification will lead to a high density of vacancies and a high volume of planar defects (stacking faults), favoring a martensitic transformation. The outcome of this work indicates that the γ to ε martensitic transformation is dominant under rapid solidification conditions with over 80 vol. % ε-HCP phase developing in most of the investigated alloys.

4.3. Mechanical Properties

From the outcome of this work, a Co-20 wt. % Cr alloy was chosen for additional testing, as this alloy exhibited minimal or no segregation with no intermetallic phases. Accordingly, the mechanical properties of this alloy were investigated before and after an isothermal heat treatment at 1003.15 K for 60 min. The heat treatment was intended to remove any internal stresses associated with the alloy rapid solidification. Figure 14 shows the effect of the isothermal heat treatment on the exhibited microstructure in the Co-20 wt. % Cr alloy. Notice that in this condition the morphology of the ε-martensite is rather different from the one in the as-cast condition, in agreement with published reports [39,40].
Figure 15a is a TEM micrograph clearly showing embedded numerous stacking faults together with various ε-martensite bands and a high density of dislocations. The corresponding diffraction pattern (Figure 15b) shows that the zone axes for the HCP ε-Co phase is now [1].
In particular, notice that the dendritic structure tends to be erased by the isothermal heat treatment. In addition, the amount of ε-martensite increases (from 85 vol. % in the as-cast condition to 96 vol. % after heat treating, see Figure 16). Apparently, under these conditions, isothermal ε-martensite develops from the athermal one and also from the remaining FCC γ-Co phase. In addition (see Figure 15a), there is an apparent thickening of ε-martensite plates and the confinement of the FCC γ-Co phase to highly localized narrow regions (see Figure 8a).
A drastic improvement in the alloy ductility was also achieved after the isothermal heat treating (i.e., up to 26% elongation), which is over a 10-fold increase when compared with the alloy in the as-cast condition [21,22,41,42]. These elongation values are rather similar to the ones reported for other Co-alloys heat treated at high temperatures [41], forged [43] or hot rolled [44], as shown in Figure 17. Notice from the fracture modes that the effect of the prior columnar dendritic structure was not dominant in the final fracture path in the heat-treated condition (see Figure 10). Moreover, the exhibited brittle fracture path in the as-cast alloy is not related to inhomogeneous solute distribution as the alloy did not exhibit any significant segregation effects nor precipitation of any intermetallic phases. Thus, the outcome of this work indicates that rapid solidification in Co-Cr alloys promotes microstructural homogeneity. Moreover, through alloy heat treating, the resultant mechanical properties are drastically improved, becoming highly attractive for potential biomedical applications.

4.4. Corrosion Properties

The experimental Co-20 wt. % Cr was found to possess an optimum combination of strength and ductility for some potential biomedical applications. Yet another critical alloy requirement is related to a high biocompatibility in the human body, particularly high corrosion resistance. Hence, preliminary testing was carried out to assess the alloy corrosion behavior. This is primarily motivated by the potentially harmful effects associated with the high cytotoxicity of the byproducts generated during the corrosion process [17]. From the corrosion results (see Figure 11 and Table 3) it was found that the corrosion properties of the Co-20 wt. % Cr alloy in the as-cast condition are slightly superior to the ones obtained after the heat treatment. In turn, this confirms that the as-cast alloy is highly homogeneous as there are no preferential defects such as intermetallics or alloy segregation that can trigger severe or localized corrosion. Moreover, in both cases, the exhibited corrosion rates are appreciably lower than the ones corresponding with those reported for other Co-Cr alloys [29] under similar corrosion conditions in artificial saliva. Thus, it is evident that through microstructural control using rapid solidification (i.e., suppression of interdendritic segregation and intermetallic precipitation) it is plausible to design a Co-Cr alloy with unique properties for applications such as in dental materials.

5. Conclusions

(1)
In this work an alternative solidification process is proposed that can be used to produce Co-Cr alloys with unique microstructures.
(2)
Through the use of wedge-shaped copper molds, rapid solidification regimes were achieved in the solidified alloys.
(3)
In the eutectic composition (Co-44 wt. % Cr alloy) there were some constitutional changes; as a result of rapid solidification, the FCC γ-Co and HCP ε-Co solid solution phases were able to form outside their equilibrium limits (solid solubility extension). In addition, dendrite refinement and elimination or reduction of interdendritic segregation for Co-20, 30, 35, 40, and 44 wt. % Cr alloys was observed, which can be considered as one of the microstructural effects due to rapid solidification.
(4)
Rapid solidification effects, such as excess vacancies and the development of numerous stacking faults and corresponding intersections, strongly favored the athermal ε-martensite transformation. Amounts of athermal ε-martensite exceeding 80 vol. % were induced at all of the cooling rates imposed on most of the alloys in the as-cast condition.
(5)
An isothermal heat treatment below the γ-ε phase transformation temperature was implemented in the Co-20 wt. % Cr alloy. In turn, the mechanical strength was found to improve by over 40% whereas the alloy ductility exhibited over a 10-fold increase when compared with the alloy in as-cast condition. SEM and TEM characterization revealed that in the as-cast condition the resultant microstructure is composed of fine athermal ε-martensite plates inside directionally solidified columnar dendrites. After aging, the morphology undergoes a change due to the isothermal transformation of HCP ε-martensite as confirmed by X-ray diffraction data.
(6)
Potentiodynamic polarization curves indicated that the Co-20 wt. % Cr alloy exhibited the lowest corrosion rates when compared with other Co-based alloys currently in use. In turn, preliminary results indicate that the combination of mechanical strength and corrosion resistance exhibited by this alloy processed by rapid solidification makes it attractive for potential applications as a biomaterial.

Acknowledgments

The authors would like to express their gratitude for the technical work of A. Tejeda, C. Flores-Morales C. Zorrilla. We acknowledge the financial support from UNAM/PAPIIT IT100316.

Author Contributions

Julio A. Juarez-Islas designed the experiments; Julio A. Juarez-Islas, Ana L. Ramirez-Ledesma and Hugo F. Lopez analyzed the results; the paper was written by all authors.

Conflicts of Interest

The authors declare no conflict of interest.

References

  1. Vandamme, N.S.; Topoleski, L.D.T. Control of surface morphology of carbide coating on Co-Cr-Mo implant alloy. J. Mater. Sci. Mater. Med. 2005, 16, 647–654. [Google Scholar] [CrossRef] [PubMed]
  2. Podrez-Radziszewska, M.; Haimann, K.; Dudziński, W.; Morawska-Sołtysik, M. Characteristic of intermetallic phases in cast dental CoCrMo alloy. Arch. Foundry Eng. 2010, 10, 51–56. [Google Scholar]
  3. Lee, S.H.; Nomura, N.; Chiba, A. Significant improvement in mechanical properties of biomedical Co-Cr-Mo alloys with combination of N addition and Cr-enrichment. Mater. Trans. JIM 2008, 49, 260–264. [Google Scholar] [CrossRef]
  4. Niinomi, M.; Nakai, M.; Hieda, J. Development of new metallic alloys for biomedical applications. Acta Biomater. 2012, 8, 3888–3903. [Google Scholar] [CrossRef] [PubMed]
  5. Hedberg, Y.S.; Qian, B.; Shen, Z.; Virtanen, S.; Odnevall-Wallinder, I. In vitro biocompatibility of CoCrMo dental alloys fabricated by selective laser melting. Dent. Mater. 2014, 30, 525–534. [Google Scholar] [CrossRef] [PubMed]
  6. Berlin, R.M.; Gustavson, L.J.; Wang, K.K. Influence of post processing on the mechanical properties of investment cast and wrought Co-Cr-Mo alloys. In Cobalt Base Alloys for Biomedical Applications; Disegi, J.A., Kennedy, R.L., Pilliar, R., Eds.; ASTM International: West Conshohocken, PA, USA, 1999; pp. 62–70. [Google Scholar]
  7. Kaiser, R.; Williamson, K.; O’Brien, C.; Browne, D.J. Effects of section size, surface cooling conditions, and crucible material on microstructure and as-cast properties of investment cast Co-Cr biomedical alloy. Metall. Mater. Trans. A 2013, 44A, 5333–5342. [Google Scholar] [CrossRef]
  8. Lee, S.H.; Takahashi, E.; Nomura, N.; Chiba, A. Effect of carbon addition on microstructure and mechanical properties of a wrought Co-Cr-Mo implant alloy. Mater. Trans. JIM 2006, 47, 287–290. [Google Scholar] [CrossRef]
  9. Salinas-Rodriguez, A.; Rodriguez-Galicia, J.L. Deformation behavior of low-carbon Co-Cr-Mo alloys for low-friction implant applications. J. Biomed. Mater. Res. 1996, 31, 409–419. [Google Scholar] [CrossRef]
  10. Mani, A.; Salinas-Rodriguez, A.; Lopez, H.F. Deformation induced FCC to HCP transformation in a Co-27Cr-5Mo-0.05C alloy. Mater. Sci. Eng. A 2011, 528A, 3037–3043. [Google Scholar] [CrossRef]
  11. Lee, S.H.; Takahashi, E.; Nomura, N.; Chiba, A. Effect of heat treatment on microstructure and mechanical properties of Ni- and C-free Co-Cr-Mo alloys for medical applications. Mater. Trans. JIM 2005, 46, 1790–1793. [Google Scholar] [CrossRef]
  12. Paul, B.; Kapoor, R.; Chakravartty, J.K.; Bidaye, A.C.; Sharma, I.G.; Suri, A.K. Hot working characteristics of cobalt in the temperature range 600–950 °C. Scr. Mater. 2009, 60, 104–107. [Google Scholar] [CrossRef]
  13. Mori, M.; Yamanaka, K.; Sato, S.; Wagatsuma, K.; Chiba, A. Microstructures and mechanical properties of biomedical Co-29Cr-6Mo-0.14N alloys processed by hot rolling. Metall. Mater. Trans. A 2012, 42A, 3108–3119. [Google Scholar] [CrossRef]
  14. ASTM F562-13. Standard Specification for Wrought 35Cobalt-35Nickel-20Chromium-10Molybdenum Alloy for Surgical Implant Applications (UNS R30035); ASTM International: West Conshohocken, PA, USA, 2013. [Google Scholar]
  15. Niinomi, M. Recent research and development in titanium alloys for biomedical applications and healthcare goods. Sci. Technol. Adv. Mater. 2003, 4, 445–454. [Google Scholar] [CrossRef]
  16. Roach, M. Base metal alloys used for dental restorations and implants. Dent. Clin. N. Am. 2007, 51, 603–627. [Google Scholar] [CrossRef] [PubMed]
  17. Saravanan, G.; Mohan, S. Structure, composition and corrosion resistance studies of Co-Cr alloy electrodeposited from deep eutectic solvent (DES). J. Alloy. Compd. 2012, 522, 162–166. [Google Scholar] [CrossRef]
  18. Taylor, R.N.J.; Waterhouse, R.B. A study of the ageing behaviour of a cobalt based implant alloy. J. Mater. Sci. 1983, 18, 3265–3280. [Google Scholar] [CrossRef]
  19. Giancchi, J.V.; Morando, C.N.; Fornaro, O.; Palacio, H.A. Microstructural characterization of as-cast biocompatible Co-Cr-Mo alloys. Mater. Charact. 2011, 62, 53–61. [Google Scholar] [CrossRef]
  20. Zhuang, L.Z.; Langer, E.W. Effects of alloy additions on the microstructures and tensile properties of cast Co-Cr-Mo alloy used for surgical implants. J. Mater. Sci. 1989, 24, 4324–4330. [Google Scholar] [CrossRef]
  21. Zhuang, L.Z.; Langer, E.W. Effects of cooling rate control during the solidification process on the microstructure and mechanical properties of cast Co-Cr-Mo alloy used for surgical implants. J. Mater. Sci. 1989, 24, 381–388. [Google Scholar] [CrossRef]
  22. Montero-Ocampo, C.; Talavera, M.; Lopez, H. Effect of alloy preheating on the mechanical properties of as-cast Co-Cr-Mo-C alloys. Metall. Mater. Trans. A 1999, 30A, 611–620. [Google Scholar] [CrossRef]
  23. Mineta, S.; Alfirano; Namba, S.; Yoneda, T.; Ueda, K. Phase and formation/dissolution of precipitates in biomedical Co-Cr-Mo alloys with nitrogen addition. Metall. Mater. Trans. A 2013, 44A, 494–503. [Google Scholar] [CrossRef]
  24. Pilliar, R.M. Metallic biomaterials. In Biomedical Materials; Narayan, R., Ed.; Springer: New York, NY, USA, 2009; pp. 41–82. [Google Scholar]
  25. Song, C.; Park, H.; Lopez, H.F. Development of athermal and isothermal ε-martensite in atomized Co-Cr-Mo-C implant alloy powders. Metall. Mater. Trans. A 2006, 37A, 3197–3204. [Google Scholar] [CrossRef]
  26. Sage, M.; Guillaud, C. Méthode d'analyse quantitative des variétés allotropiques du cobalt pre les Rayons X. Rev. Metall. 1950, 49, 139–145. [Google Scholar]
  27. Shi, L.; Northwood, D.O.; Cao, Z. Alloy design and microstructure of a biomedical Co-Cr alloy. J. Mater. Sci. 1993, 28, 1312–1315. [Google Scholar] [CrossRef]
  28. Huang, P.; Lopez, H.F. Strain induced ε-martensite in a Co-Cr-Mo alloy: Grain size effects. Mater. Lett. 1999, 39, 244–248. [Google Scholar] [CrossRef]
  29. Yamanaka, K.; Mori, M.; Chiba, A. Enhanced Mechanical Properties of As-Forged Co-Cr-Mo-N Alloys with Ultrafine-Grained Structures. Metall. Mater. Trans. A 2012, 43A, 5243–5257. [Google Scholar] [CrossRef]
  30. Sharma, M.; Ramesh-Kumar, A.V.; Singh, N.; Adya, N.; Saluja, B. Electrochemical corrosion behavior of dental/implant alloys in artificial saliva. J. Mater. Eng. Perform. 2008, 17, 695–701. [Google Scholar] [CrossRef]
  31. Angelini, E.; Zucchi, F. In vitro corrosion of some Co-Cr and Ni-Cr alloys used for removable partial dentures: Influence of heat treatments. J. Mater. Sci. Mater. Med. 1991, 2, 27–35. [Google Scholar] [CrossRef]
  32. Tomas, H.; Freire, A.P.; Abrantes, L.M. Cast Co-Cr alloy and pure chromium in proteinaceous media: An electrochemical characterization. J. Mater. Sci. Mater. Med. 1994, 5, 446–451. [Google Scholar] [CrossRef]
  33. Lawrence-Kats, J. Orthopedic applications. In Biomaterials Science: An Introduction to Materials in Medicine; Ratner, B.D., Hoffman, A.S., Schoen, F.J., Lemons, J.E., Eds.; Elsevier: London, UK, 2004; pp. 335–346. [Google Scholar]
  34. Bogno, A.; Nguyen-Thi, H.; Reinhart, G.; Billia, B.; Baruchel, J. Growth and interaction of dendritic equiaxed grains: In situ characterization by synchrotron X-ray radiography. Acta Mater. 2013, 61, 1302–1315. [Google Scholar] [CrossRef]
  35. Lopez, H.F.; Saldivar, A.; Huang, P. Development and properties of ε-martensite in Co-Cr-Mo alloys for biomedical applications. In Properties of Complex Inorganic Solids 2; Meike, A., Gonis, A., Turchi, P., Rajan, K., Eds.; Kluwer Academic/Plenum Publishers: New York, NY, USA, 1999; pp. 307–325. [Google Scholar]
  36. Huang, P.; Salinas-Rodriguez, A.; Lopez, H.F. Tribological behaviour of cast and wrought Co-Cr-Mo implant alloys. Mater. Sci. Technol. 1999, 15, 1324–1330. [Google Scholar]
  37. Saldivar-Garcia, A.; Mani-Medrano, A.; Salinas-Rodriguez, A. Effect of solution treatments on the fcc/hcp isothermal martensitic transformation in Co-27Cr-5Mo-0.05C aged at 800 °C. Scr. Mater. 1999, 40, 717–722. [Google Scholar] [CrossRef]
  38. Rajan, K. Phase Transformations in a Wrought Co-Cr-Mo-C Alloy. Metall. Mater. Trans. A 1982, 13A, 1161–1166. [Google Scholar] [CrossRef]
  39. Jones, H. Rapid Solidification of Metals and Alloys; The Institution of Metallurgists: London, UK, 1982; pp. 1–80. [Google Scholar]
  40. Saldivar, A.J.; Lopez, H.F. Role of aging on the martensitic transformation in a cast cobalt alloy. Scr. Mater. 2001, 45, 427–433. [Google Scholar] [CrossRef]
  41. Saldivar-Garcia, A.J.; Mani-Medrano, A.; Salinas-Rodriguez, A. Formation of Hcp martensite during the isothermal aging of an Fcc Co-27Cr-5Mo-0.05C orthopedic implant alloy. Metall. Mater. Trans. A 1999, 30A, 1177–1184. [Google Scholar] [CrossRef]
  42. Vander-Sande, J.B.; Coke, J.R.; Wulff, J. A transmission electron microscopy the mechanisms of strengthening in heat-treated Co-Cr-Mo-C alloys. Metall. Mater. Trans. A 1976, 7A, 389–397. [Google Scholar] [CrossRef]
  43. Lashgari, H.R.; Zangeneh, S.; Hasanabadi, F.; Saghafi, M. Microstructural evolution during isothermal aging and strain-induced transformation followed by isothermal aging in Co-Cr-Mo-C alloy: A comparative study. Mater. Sci. Eng. A 2010, 527A, 4082–4091. [Google Scholar] [CrossRef]
  44. Chiba, A.; Kumagai, K.; Takeda, H.; Nomura, N. Mechanical properties of forged low Ni and C-containing Co-Cr-Mo. Mater. Sci. Forum 2005, 475–479, 2317–2322. [Google Scholar] [CrossRef]
Figure 1. (a) Wedge-shaped copper mold isolated in both sides by an alumina sheet; (b) “V” shaped ingot showing three different cooling rate zones: 90 mm high: 120 K/s, 60 mm high: 230 K/s, and 20 mm high: 450 K/s.
Figure 1. (a) Wedge-shaped copper mold isolated in both sides by an alumina sheet; (b) “V” shaped ingot showing three different cooling rate zones: 90 mm high: 120 K/s, 60 mm high: 230 K/s, and 20 mm high: 450 K/s.
Metals 06 00188 g001
Figure 2. (a) Representative cooling curves exhibited at various locations. (1) Tip; (2) middle; (3) top in a chill-cast wedge of Co-20 wt. %Cr alloy. In the inset two solid state events can be seen: (1) the martensitic transformation at 868 °C; and (2) Co3Cr precipitation at 538 °C; (b) exhibited microstructures for the Co-20, 30, 35, 40, and 44 wt. % Cr, along the wedge-shaped ingot.
Figure 2. (a) Representative cooling curves exhibited at various locations. (1) Tip; (2) middle; (3) top in a chill-cast wedge of Co-20 wt. %Cr alloy. In the inset two solid state events can be seen: (1) the martensitic transformation at 868 °C; and (2) Co3Cr precipitation at 538 °C; (b) exhibited microstructures for the Co-20, 30, 35, 40, and 44 wt. % Cr, along the wedge-shaped ingot.
Metals 06 00188 g002
Figure 3. Microstructures found in wedge shaped Co-Cr alloy ingots. (a) Co-20 wt. % Cr; (b) Co-30 wt. % Cr; (c) Co-35 wt. % Cr; (d) Co-40 wt. % Cr; and (e) Co-44 wt. % Cr. It is important to note that the heat flux direction is always in the opposite sense with respect to the columnar dendrites growth.
Figure 3. Microstructures found in wedge shaped Co-Cr alloy ingots. (a) Co-20 wt. % Cr; (b) Co-30 wt. % Cr; (c) Co-35 wt. % Cr; (d) Co-40 wt. % Cr; and (e) Co-44 wt. % Cr. It is important to note that the heat flux direction is always in the opposite sense with respect to the columnar dendrites growth.
Metals 06 00188 g003
Figure 4. Interdendritic segregation reported in Co-alloys. References are given in parentheses and the chill cast corresponds to the present work.
Figure 4. Interdendritic segregation reported in Co-alloys. References are given in parentheses and the chill cast corresponds to the present work.
Metals 06 00188 g004
Figure 5. Representative X-ray diffraction patterns for the Co-Cr alloys: (a) Co-20 wt. % Cr; (b) Co-30 wt. % Cr; (c) Co-35 wt. % Cr; (d) Co-40 wt. % Cr at the center of the wedge-shaped cooper mold.
Figure 5. Representative X-ray diffraction patterns for the Co-Cr alloys: (a) Co-20 wt. % Cr; (b) Co-30 wt. % Cr; (c) Co-35 wt. % Cr; (d) Co-40 wt. % Cr at the center of the wedge-shaped cooper mold.
Metals 06 00188 g005
Figure 6. Percent of ε-phase as a function of alloy processing.
Figure 6. Percent of ε-phase as a function of alloy processing.
Metals 06 00188 g006
Figure 7. As-cast Co-20 wt. % Cr microstructure: scanning electron microscope (SEM) micrograph of the FCC γ-Co dendrites and athermal ε-martensite formed inside the dendrites.
Figure 7. As-cast Co-20 wt. % Cr microstructure: scanning electron microscope (SEM) micrograph of the FCC γ-Co dendrites and athermal ε-martensite formed inside the dendrites.
Metals 06 00188 g007
Figure 8. As-cast Co-20 wt. % Cr: (a) transmission electron microscope (TEM) micrograph showing the presence of FCC γ-Co phase between the ε-martensite plates; (b) corresponding electron diffraction pattern.
Figure 8. As-cast Co-20 wt. % Cr: (a) transmission electron microscope (TEM) micrograph showing the presence of FCC γ-Co phase between the ε-martensite plates; (b) corresponding electron diffraction pattern.
Metals 06 00188 g008
Figure 9. Stress-strain curves for Co-20 wt. % Cr alloy: (a) in the as-chill cast condition and (b) heat-treated condition.
Figure 9. Stress-strain curves for Co-20 wt. % Cr alloy: (a) in the as-chill cast condition and (b) heat-treated condition.
Metals 06 00188 g009
Figure 10. Fractography of Co-20 wt. % Cr alloy: (a) in the as-chill cast condition and (b) heat-treated condition.
Figure 10. Fractography of Co-20 wt. % Cr alloy: (a) in the as-chill cast condition and (b) heat-treated condition.
Metals 06 00188 g010
Figure 11. Polarization curves for the Co-20 wt. % Cr alloys in both, the as-chill cast and the heat treated conditions.
Figure 11. Polarization curves for the Co-20 wt. % Cr alloys in both, the as-chill cast and the heat treated conditions.
Metals 06 00188 g011
Figure 12. Mapping of the various phases found including intermetallics and the eutectic constituent as a function of cooling rates and % Cr.
Figure 12. Mapping of the various phases found including intermetallics and the eutectic constituent as a function of cooling rates and % Cr.
Metals 06 00188 g012
Figure 13. (a) SEM micrograph of the as-chill cast Co-20 wt. % Cr directionally solidified alloy showing a part of columnar dendrites, (b) X-ray mapping of Cr (chromium).
Figure 13. (a) SEM micrograph of the as-chill cast Co-20 wt. % Cr directionally solidified alloy showing a part of columnar dendrites, (b) X-ray mapping of Cr (chromium).
Metals 06 00188 g013
Figure 14. As-heat-treated microstructure showing isothermally developed HCP ε-Co plates.
Figure 14. As-heat-treated microstructure showing isothermally developed HCP ε-Co plates.
Metals 06 00188 g014
Figure 15. Heat-treated Co-20 wt. %Cr: (a) TEM micrograph showing HCP ε-Co plates and (b) corresponding electron diffraction pattern.
Figure 15. Heat-treated Co-20 wt. %Cr: (a) TEM micrograph showing HCP ε-Co plates and (b) corresponding electron diffraction pattern.
Metals 06 00188 g015
Figure 16. Diffraction patterns of Co-20 wt. % Cr alloy: (a) as-chill cast condition; (b) heat-treated condition.
Figure 16. Diffraction patterns of Co-20 wt. % Cr alloy: (a) as-chill cast condition; (b) heat-treated condition.
Metals 06 00188 g016
Figure 17. Percent elongation of Co-alloys as a function of alloy processing.
Figure 17. Percent elongation of Co-alloys as a function of alloy processing.
Metals 06 00188 g017
Table 1. Chemical composition of the artificial saliva.
Table 1. Chemical composition of the artificial saliva.
CompoundQuantity (g/L)
KH2PO40.34
Na2HPO4·2H2O0.445
KHCO31.5
NaCl0.585
MgCl2·6H2O0.0305
Citric acid0.0315
CaCl20.0166
Table 2. Athermal ε-martensite transformation as a function of cooling rates for several Cr contents.
Table 2. Athermal ε-martensite transformation as a function of cooling rates for several Cr contents.
Cr (wt. %)Cooling Rate (K/s)HCP (wt. %)I(l0Īl)HCPI (200)FCC
2045082.3184.2226.32
23089.6277.9221.32
12092.6481.8225.32
3045061.638.37215.92
23090.177.325.62
12081.192.9214.32
3545079.090.3215.92
23092.1200.5211.32
12081.9145.5221.32
4045081.951.327.52
23043.8166.72142.22
12051.525.1215.72
Table 3. Electrochemical parameters obtained from the polarization curves of Co-20 wt. % Cr alloys polarized in Artificial Saliva Solution.
Table 3. Electrochemical parameters obtained from the polarization curves of Co-20 wt. % Cr alloys polarized in Artificial Saliva Solution.
Co-20 wt. % Cr (Condition)Ecorr (mV)Icorr (mA/cm2)Epit (mV)Ipit (mA/m2)Vcorr (mm/year)
As-cast (present work)−554.21 × 10−4298.20.0060.00084
Heat treated−524.194.22 × 10−4384.160.0140.00356
(present work)
Co-Cr as-cast [17] 1.26
Co-Cr as-cast [29] 5.43
Co-Cr Heat treated [29] 0.061

Share and Cite

MDPI and ACS Style

Ramirez-Ledesma, A.L.; Lopez, H.F.; Juarez-Islas, J.A. Evaluation of Chill Cast Co-Cr Alloys for Biomedical Applications. Metals 2016, 6, 188. https://doi.org/10.3390/met6080188

AMA Style

Ramirez-Ledesma AL, Lopez HF, Juarez-Islas JA. Evaluation of Chill Cast Co-Cr Alloys for Biomedical Applications. Metals. 2016; 6(8):188. https://doi.org/10.3390/met6080188

Chicago/Turabian Style

Ramirez-Ledesma, Ana Laura, Hugo F. Lopez, and Julio Alberto Juarez-Islas. 2016. "Evaluation of Chill Cast Co-Cr Alloys for Biomedical Applications" Metals 6, no. 8: 188. https://doi.org/10.3390/met6080188

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.

Article Metrics

Back to TopTop