Next Article in Journal
The Effect of Poly (Ethylene glycol) Emulation on the Degradation of PLA/Starch Composites
Next Article in Special Issue
Paper Ageing: The Effect of Paper Chemical Composition on Hydrolysis and Oxidation
Previous Article in Journal
Finite Element Method-Based Simulation Creep Behavior of Viscoelastic Carbon-Fiber Composite
Previous Article in Special Issue
Rendering Banana Plant Residues into a Potentially Commercial Byproduct by Doping Cellulose Films with Phenolic Compounds
 
 
Font Type:
Arial Georgia Verdana
Font Size:
Aa Aa Aa
Line Spacing:
Column Width:
Background:
Article

Semi-Crystalline Hydrophobic Polyamidoamines: A New Family of Technological Materials?

1
Dipartimento di Chimica, Università Degli Studi di Milano, via C. Golgi 19, 20133 Milano, Italy
2
Dipartimento di Scienza Applicata e Tecnologia, Politecnico di Torino, Alessandria Campus, Viale T. Michel, 15121 Alessandria, Italy
3
Istituto Polimeri, Compositi e Biomateriali (IPCB), Consiglio Nazionale Delle Ricerche, via Campi Flegrei 34, 80078 Pozzuoli, Italy
*
Authors to whom correspondence should be addressed.
Polymers 2021, 13(7), 1018; https://doi.org/10.3390/polym13071018
Submission received: 2 March 2021 / Revised: 20 March 2021 / Accepted: 22 March 2021 / Published: 25 March 2021
(This article belongs to the Special Issue Feature Papers of Green and Sustainable Chemistry in Polymer Science)

Abstract

:
The hitherto known polyamidoamines (PAAs) are not suitable as structural materials because they are usually water-soluble or swellable in water. This paper deals with the synthesis and characterization of semi-crystalline hydrophobic PAAs (H-PAAs) by combining different bis-sec-amines with bis-acrylamides obtained from C6–C12 bis-prim-amines. H-PAAs were initially obtained in a solution of benzyl alcohol, a solvent suitable for both monomers and polymers. Their number average molecular weights, M ¯ n , which were determined with 1H-NMR by evaluating the percentage of their terminal units, varied from 6000 to >10,000. The solubility, thermal properties, ignitability and water resistance of H-PAAs were determined. They were soluble in organic solvents, semi-crystalline and thermally stable. The most promising ones were also prepared using a bulk process, which has never been previously reported for PAA synthesis. In the form of films, these H-PAAs were apparently unaffected by water. The films underwent tensile and wettability tests. They showed similar Young moduli (260–263 MPa), whereas the maximum stress and the stress at break depended on the number of methylene groups of the starting bis-acrylamides. Their wettability was somewhat higher than that of common Nylons. Interestingly, none of the H-PAAs considered, either as films or powders, ignited after prolonged exposure to a methane flame.

Graphical Abstract

1. Introduction

Linear polyamidoamines (PAAs) are synthetic polymers obtained from the aza-Michael polyaddition of prim-monoamines or bis-sec-amines with bis-acrylamides [1,2,3]. The reaction is specific since other chemical functions, except thiols and prim- or sec-phosphine groups, do not participate in it. Nearly all bis-acrylamides, bis-sec-amines and prim-amines available on the market or described in the literature are potential monomers. Consequently, PAAs are a polymer class with high structural versatility. In particular, they can be designed to be biocompatible and degradable [4,5,6]. All PAAs described so far are highly hydrophilic and in most cases water soluble. Many of them have shown potential as complexing agents of heavy metal ion [7], constituents of sensors [8,9,10], heparin complexing agents [11,12,13], drug carriers [14,15,16], antiviral drugs [17,18] and transfection promoters [19,20,21,22]. Proteins graft copolymers have been also described [23].
Cross-linked PAAs are obviously insoluble but swell in water giving hydrogels. Some of these hydrogels proved good scaffolds [24,25,26] for cell culture and promoted cell adhesion and proliferation both in vitro and in vivo. In the form of tubes, they acted as excellent resorbable scaffolds for sciatic nerve regeneration in rats [24]. Undoubtedly, these properties were mediated by their positive charge at the physiological pH which, however, was too low to elicit cellular toxicity. PAA hydrogels showed poor mechanical properties when swollen in water and were hard and brittle when dry. This has hampered their widespread use as implantable biomaterials. To overcome this problem, several approaches have been investigated, such as the preparation of PAA nanocomposite hydrogels with biocompatible nanosized inorganic fillers, such as montmorillonite [27], or their reinforcement with nanofibrous PLLA (poly(L-lactic acid)) mats previously aminated by plasma treatment with nitrogen [28]. In the latter case, the hydrogels were synthesized by embedding the PLLA mat in the curing solution. The amino groups present on the PLLA fibers participated in the polyaddition reaction and gave rise to matrix-fiber covalent bonds, which ensured the stability of the composite in water. Both approaches were only partially successful. Inorganic nanofillers greatly improved the overall mechanical properties of PAA hydrogels but failed to make them susceptible to being attached to body tissues by stitching. As for the PLLA reinforced composite hydrogels, their preparation was difficult to scale up. So far, no attempts have been made to obtain PAAs inherently endowed with potential as structural materials. This paper aims to fill this gap by reporting the synthesis and properties of a small library of hitherto undescribed semi-crystalline hydrophobic PAAs (H-PAAs) that show promise in this regard.

2. Materials and Methods

Materials. Acryloyl chloride (97%), sodium hydroxide (>98%), 1,6-hexanediamine (98%), 1,8-octanediamine (98%), 1,10-decanediamine (98%), 1,12-dodecanediamine (≥97%), 2,6-di-tert-butyl-p-cresol (≥99%), N,N’-dimethylethylenediamine (DM2) (99%), N,N’-dimethyl-1,6-hexanediamine (DM6) (97%), N,N’-diethylethylenediamine (DE2) (95%), N,N’-dibenzylethylenediamine (DB2) (97%), piperazine (PIP) (99%), benzyl alcohol (≥99.8%), alcohol-free chloroform (≥99.8%), diethyl ether (≥99%), CDCl3 (99.8%), CD3OD (99.96%), D2O (99.9%) and CD3COOD (99.9%) were purchased from Sigma-Aldrich (Milano, Italy) and used as received.
Synthetic procedures. N,N’-Dodecamethylene-bis-acrylamide (B12). In a 1 L four-necked round bottom flask, equipped with a thermometer, a mechanical stirrer and two dropping funnels, 1,12-dodecanediamine (31.0 g, 150.0 mmol) was suspended in CHCl3 (800 mL). Under vigorous stirring, the suspension was cooled to 0 ± 1 °C with an acetone/ice bath. Acryloyl chloride (27.6 mL, 329.5 mmol) in CHCl3 (18 mL) and NaOH (13.8 g, 338.1 mmol) in H2O (34 mL) solutions were added dropwise, maintaining the temperature at around 0–2 °C. At the end of the addition, the reaction mixture was allowed to warm up to room temperature and stirred for 24 h. The solid formed was filtered, washed with an acetic acid/H2O 1:2 v/v solution (270 mL), then with H2O until neutral pH. The resulting product was an off-white solid, which was dried under a vacuum to constant weight (Fraction “a”). Yield: 24.9 g (54.0%). An additional crop was recovered by evaporating the mother liquors to dryness, washing the solid residue with 30% aqueous acetic acid (40 mL) and then water until neutral pH, and drying to constant weight under a vacuum (Fraction “b”). Yield: 2.8 g. The 1H-NMR and FT-IR spectra of the two fractions demonstrated that they were identical.
All other bis-acrylamides were prepared following the same procedure adopted for B12. The amounts of amine used and the yields are reported in Table 1.
Synthesis of B6-DM2 by the solution process. N,N’-Hexamethylene-bis-acrylamide (11.2 g, 50 mmol), N,N’-dimethylethylenediamine (4.5 g, 50 mmol) and benzyl alcohol (46 mL) were introduced into a 100 mL screw cap tube, and the mixture was stirred magnetically at 60 °C for 48 h. The reaction mixture gradually became homogeneous. The solution was finally cooled down to room temperature, precipitated in diethyl ether (500 mL) under stirring and kept at about 5–8 °C overnight. The final product was retrieved by filtering and dried under a vacuum as a whitish solid. Yield 13.3 g (85%).
All other polymers were prepared as described for B6-DM2 using the amounts of reagents and solvent reported in Table 2.
Synthesis of H-PAAs by the bulk process. B12-DM6. N,N’-dimethyl-1,6-hexanediamine (15.4 g, 50 mmol), N,N’-dodecamethylene-bis-acrylamide (7.4 g, 32.4 mmol) and 2,6-di-tert-butyl-p-cresol (150 mg) were introduced into a hermetically sealed cylindrical glass reactor equipped with a thermocouple, a nitrogen inlet and a u-shaped mechanical paddle stirrer. After carefully flushing with nitrogen, the reaction mixture was heated up to 70 °C while homogenizing under stirring. The temperature was then raised up to 140 °C within 1 h and maintained at a constant for further 2 h. After this time, the reacting mixture was allowed to cool down to room temperature. The solidified product was retrieved as a yellowish solid. The yield was quantitative, apart from mechanical losses.
B8-DM6 was prepared as described for B12-DM6, by substituting N,N’-octamethylene-bis-acrylamide (12.4 g) for N,N’-dodecamethylene-bis-acrylamide and heating up to 150 °C.
Solubility tests. H-PAA solubility was determined in a step-by-step procedure. Polymer samples (5 mg) were dispersed in 0.5 mL of solvent and kept under stirring for 15 min. The samples that did not give a clear solution were heated to the solvent boiling point, and the solubility was ascertained. If insoluble, the solutions were diluted with additional solvent (0.5 mL) and the procedure was repeated.
Nuclear magnetic resonance. The chemical structure of monomers and polymers was assessed by 1H-NMR spectroscopy using a Bruker Avance DPX-400 NMR spectrometer (Milano, Italy) operating at 400.13 MHz. The spectra of bis-acrylamides were collected in CD3OD and those of H-PAAs in CDCl3 at 25 °C.
Thermal properties. Thermogravimetric analyses (TGA) were performed from 35 to 800 °C in both air and nitrogen on a Mettler-Toledo TGA/DSC 2 Star System instrument (Milano, Italy). Samples (5–10 mg) were placed in alumina crucibles and heated at a 10 °C min−1 heating rate under a 50 mL min−1 nitrogen flow.
Differential scanning calorimetric (DSC) analyses were performed on a Mettler-Toledo DSC823e System (Milano, Italy) as follows: samples (5 mg) were placed in standard aluminum crucibles and heated or cooled at 5 °C min−1 under an 80 mL min−1 nitrogen flow. The heating program was as follows: 1st step: heating from 25 °C to Tf; 2nd step: 1 min at Tf; 3rd step: cooling from Tx to 25 °C; 4th step: 1 min at 25 °C; 5th step: heating from 25 °C to Tx; 6th step: 1 min at Tf; 7th step: cooling from Tx to 25 °C. Tf is the maximum temperature typical of each polymer. Result accuracy was ±1 °C and ±0.01 J g−1. Before ea ch set of analyses, the instrument was calibrated with an indium standard. Tg values were assessed by a TA Waters instrument Model DSCQ20 (Milano, Italy); samples (5.5 mg) were placed in standard aluminum crucibles and heated or cooled at 10 °C min−1 under a 80 mL min−1 nitrogen flow. The heating program was as follows: 1st step: heating from 25 °C to Tf; 2nd step: 1 min at Tf; 3rd step: cooling from Tx to −50 °C; 4th step: 1 min at −50 °C; 5th step: heating from −50 °C to Tx.
Ignitability. The ignitability of H-PAAs was assessed by applying a methane flame (20 mm long) directly to the polymer powder (~500 mg) placed on a ceramic-porcelain spoon spatula for 10 s, as already done for other flame retardants [29].
Preliminary evaluation of resistance to handling and to water contact of H-PAA films. Films 0.2 Mm thick were obtained by melting polymer samples (100 mg) on a heating plate in a 5 cm2 frame at a temperature of 20 °C above their melting point, then pressing with a 1.5 Kg weight for 10 s at the same temperature and finally cooling to room temperature. One half of the films obtained were incubated in water for 1 min, and the handling resistance was compared with that of the corresponding dry films.
Tensile properties. Tensile stress-strain tests were performed according to the ISO 37-2011 standard. bB12-DM6 and bB8-DM6 films 1 mm thick were obtained using a compression molding press (Model C, Carver Laboratory Press, Wabash, IN, USA). The samples (2 g) were first dried at 60 °C overnight in a vacuum oven, then placed between two pre-heated steel plates at the desired temperature (110 °C for B12-DM6 and 120 °C for B8-DM6) and finally subjected to 0.5 ton (191,406 Pa) for 4 min and then to 0.8 ton (306,250 Pa) for 1 min. The samples were then cooled to room temperature using circulating water. From this process, films 0.1 mm thick were obtained. The specimens for the tensile test were obtained using a specific dumbbell (dog-bone like) (total length 70 mm, central zone 25 mm). The samples were conditioned for at least 40 h at 25 °C and 50% relative humidity. Film thickness was measured at three random points using a micrometer, and the result was expressed as an average value. Tensile strength was measured with an INSTROM 5564 dynamometer (Torino, Italy), using a 1 KN load cell and a 2 mm min−1 deformation speed. Several replicate measurements (5–10) were performed on each H-PAA sample.
Wettability. Water contact angle measurements were performed with the contact angle system FTA 1000 B CLASS (First Ten Angstroms St. Johns Innovation Center, Cowley Road, Cambridge CB4 OWS, UK) according to the following protocol: deionized water drops of 30 ± 2 μL in volume were cast on a flat portion of H-PAA film. The shape of the drop was recorded with a high-speed framing camera. The contact angle was assessed by measuring the angle formed between the substrate surface and the tangent drawn from the edge of the drop. Measurements were taken after a static time of 30 s. Contact angles were measured at two points, i.e., near the center and near the edge of the specimens.

3. Results and Discussion

As stated in the introduction, the aim of this work was to prepare linear semi-crystalline hydrophobic PAAs (H-PAAs) endowed with potential as structural materials in terms of processability and fair mechanical properties. For this purpose, a small library of H-PAAs was prepared from the aza-Michael polyaddition of four α,ω-bis-acrylamides obtained from linear aliphatic C6-C12 bis-prim-amines and several bis-sec-amines, including linear α,ω-aliphatic N-substituted bis-sec-amines; a cyclic bis-sec-amine, namely piperazine; and an α,ω-arylalkyl N-substituted bis-sec-amine, namely N,N’-dibenzylethylenediamine. Regardless of the aliphatic portion, prim-amines were not considered in this study, as preliminary experiments invariably resulted in amorphous and sticky polymers.

3.1. Synthesis of Hydrophobic Bis-Acrylamides

All bis-acrylamides used, i.e., N,N’-dodecamethylene-bis-acrylamide (B12), N,N’-decamethylene-bis-acrylamide (B10), N,N’-octamethylene-bis-acrylamide (B8) and N,N’-hexamethylene-bis-acrylamide (B6) (Table 1), were synthesized by the Schotten-Baumann reaction [30,31,32]. A solution of acryloyl chloride in alcohol-free chloroform and an aqueous sodium hydroxide solution were added dropwise with vigorous stirring to a solution or fine suspension of the diamine in chloroform (Scheme 1). The reaction mixture was kept below 5 °C under stirring throughout the reaction process. The final product, precipitated as a solid and after filtration, was repeatedly washed with dilute acetic acid and then water to remove any traces of unreacted diamine. The chloroform mother liquors were first dried with anhydrous sodium sulphate and then evaporated under a vacuum. A second crop of product was recovered, and the residue was washed with dilute acetic acid and then water. Yields ranged from 60 to 70%.
The structures of all bis-acrylamides were confirmed by 1H-NMR spectroscopy. As an example, the 1H-NMR spectrum of B12, performed on CD3OD, is reported in Figure 1, while the spectra of all other bis-acrylamides are reported in Figures S1–S3. It may be observed that no separate signals for N-H amidic protons can be identified in the 1H-NMR spectrum of B12 reported in Figure 1. This may be due to different reasons, either rapid proton-deuterium exchange with the relatively acid O-D group of CD3OD or, as frequently observed, the N-H resonance peak may be very broad and hidden by overlapping with other signals.

3.2. Synthesis of H-PAAs by the Solution Process

Twelve not previously described H-PAAs (Table 3) were obtained first by solution polymerization, which is the common synthetic procedure of PAAs reported so far, by combining the bis-acrylamides B6, B8, B10 and B12 (Table 2, Section 2. Materials and Methods) with the five bis-sec-amines reported in Scheme 2.
Specifically, B12 and B6 were combined with all five bis-sec-amines, while, for comparison purposes, B10 and B8 were only combined with N,N’-dimethyl-1,6-hexanediamine (DM6). The aza-Michael polyaddition requires solvents with mobile hydrogens, such as water and alcohols, which in principle are poor solvents for hydrophobic polymers. Benzyl alcohol has been shown to be a good reaction medium for both precursor monomers and H-PAAs. All solution polymerization experiments were conducted at 60 °C. The resulting polymers were finally isolated by precipitating with ether. This process required large volumes of solvents, longer reaction times and tedious procedures to remove benzyl alcohol.
All H-PAAs were characterized by 1H-NMR and FT-IR/ATR spectroscopies. As an example, the 1H-NMR spectrum of B12-DM2 performed on CDCl3 is reported in Figure 2, while the 1H-NMR spectra of all other H-PAAs are reported in Figures S4–S14. The FT-IR spectra of all H-PAAs are reported in Figures S17–S27.
All characterizations were in agreement with the proposed structures, apart from the fact that all 1H-NMR spectra revealed the presence of a benzyl alcohol residue (1–3% w/w). This was taken into account in the interpretation of the TGA analyses (see below). The 1H-NMR spectra allowed us to estimate the number average molecular weights, M ¯ n , of the H-PAAs (see Table 2, Section 2. Materials and Methods) from the ratio between the integrals of the resonance peaks relative to the terminal units and the integrals of the resonance peaks relative to the internal repeating units. Size exclusion chromatography proved inadequate for determining the molecular weights of H-PAAs because they were strongly retained by the stationary phase, regardless of the mobile phases used. It can be seen that the 1H-NMR spectra of B12-DB2 (Figure S5) and B6-DB2 (Figure S12), both derived from N,N’-dibenzylethylenediamine, showed significant amounts of residual double bonds, and their M ¯ n values were less than 3000. Furthermore, even considering that these polymers were soft and sticky, they were not further considered.
Regarding solubility properties, it can be observed that, apart from the piperazine-based samples B12-PIP and B6-PIP, all H-PAAs had similar solubility properties (Table 4). They were completely soluble in chlorinated solvents and boiling alcohols but insoluble in ethers, acetone, dimethyl sulfoxide, water and 30% aqueous acetic acid. In contrast, both B12-PIP and B6-PIP were insoluble in chlorinated solvents and boiling alcohols but soluble in dilute acetic acid.

3.3. Synthesis of H-PAAs by the Bulk Process

A preliminary screening (see below) resulted in the selection of B12-DM6 and B8-DM6 as the best-performing H-PAAs, which were successfully synthesized even following a bulk process. Mixtures of equimolar monomers, added with a radical polymerization inhibitor, were gradually heated under stirring in nitrogen from 70 to 140 °C and then kept at the latter temperature for 2 h. The reaction mixture was then cooled down and the product used as retrieved. The resulting products, named bB12-DM6 and bB8-DM6, were characterized by 1H-NMR spectroscopy (Figures S15 and S16). Aside from the obvious absence of solvent impurities, their spectra were nearly identical to those of B12-DM6 and B8-DM6. The M ¯ n values of bB12-DM6 and bB8-DM6 were of the same order as those of B12-DM6 and B8-DM6. Advantages of the bulk process were that it was much faster than the solution process and avoided the presence of residual solvent. To the best of our knowledge, no examples of PAA synthesis by a bulk polymerization process have been reported so far.

3.4. Thermal Stability of H-PAAs

Figure 3 shows the TGA thermograms of H-PAAs conducted on both nitrogen and air in the temperature range of 150–700 °C. Table 5 reports the onset decomposition temperature at 10% weight loss, Tonset10%; the temperatures at maximum weight loss rate, Tmax1, Tmax2 and Tmax3; and the residual mass fractions measured at 400 and 550 °C, RMF400 and RMF550. Consistent with what was previously reported for hydrophilic PAAs studied as flame retardants for cotton [29], H-PAAs showed complex multimodal weight-loss curves in both nitrogen and air, deriving from a multistep degradation mechanism. All considered, H-PAAs were characterized by fairly high thermal stability in both atmospheres—higher overall than those of linear water-soluble PAAs—as evidenced by the Tonset10% and Tmax values. In particular, the Tonset10% values of all the considered H-PAAs were >265 °C in nitrogen and >266 °C in air, while the Tmax1 values were 280 °C in nitrogen and 290 °C in air.
In nitrogen, the Tonset10% values of H-PAAs derived from the same bis-acrylamide (B12 or B6) decreased by varying the structure of bis-sec-amine in the order PIP > DE2 > DM2 > DM6. Furthermore, all H-PAAs, regardless of composition, underwent two main decomposition steps in the ranges of 250–350 °C and 350–500 °C. The RMF400 values were in all cases relevant. In particular, as regards H-PAAs derived from the same bis-sec-amine, i.e., DM6, and different bis-acrylamides, it was found that the longer the bis-acrylamide hydrocarbon chain, the higher the RMF400 value, i.e., 43, 39, 33 e 23% for B12-DM6, B10-DM6, B8-DM6 and B6-DM6, respectively (Figure 3a). Regarding the dependence of RMF400 on the structure of the bis-sec-amine moieties in combination with the same bis-acrylamide, no clear correlation was observed (Figure 3c,e). Negligible (<1%) RMF was observed for all H-PAAs from 500 °C and above.
In air, both Tonset10% and Tmax2 values did not differ significantly from those observed in nitrogen, whereas the Tmax1 values were 2–32 °C lower than in nitrogen, with the sole exception of B12-DE2, whose Tmax1 was 10 °C higher. Furthermore, in the range of 300–450 °C, all H-PAAs showed a lower weight loss rate in air than in nitrogen and, as a result, the RMF400 values were remarkably higher. This has been attributed to the phenomenon of intumescence, which occurs by heating the air and is recognized as a characteristic of PAAs [29]. In air, as in nitrogen, the RMF400 values of H-PAA derived from DM6 increased with the increase in the bis-acrylamide hydrocarbon chain length, i.e., they were 61, 57, 52 and 43% for B12-DM6, B10-DM6, B8-DM6 and B6-DM6 (Figure 3b). No clear correlation between RMF400 values and the structure of the amine moiety was found (Figure 3d,f). In addition to the decomposition steps observed in nitrogen in the temperature ranges of 250–350 °C and 350–500 °C, a third decomposition step was observed in the range of 500–650 °C. RMF550 values were between 10 and 13%, while in nitrogen they were less than 1%, and almost vanished above 600–650 °C.
The thermal data of bB12-DM6 and bB8-DM6 in air and nitrogen, prepared by the bulk process, were almost superimposable to those of samples obtained from the solution process (Figure S30 for B12-DM6).
Comparing the thermal data of H-PAAs with those of common commercial polymers, it was observed that the Tonset10% and Tmax of H-PAAs did not differ significantly when switching from air to nitrogen, while those of PP [35] and HDPE [35,36] were about 50–150 °C lower in air than in nitrogen. Furthermore, above Tmax, the RMF of PE and PP in the air drops to a negligible amount. In contrast, in air H-PAAs showed a substantial RMF (15–30%) up to 500–650 °C, where a third Tmax occurred. It may be observed that the Tonset10% values of polybutylene terephthalate (PBT) [37], polyethylene terephthalate (PET) [38,39] and nylon 6 (PA6) [40,41] were higher than those of H-PAAs. Furthermore, they showed a single Tmax value, while H-PAAs showed two Tmax values, the first lower than- and the second, comparable to those of PBT, PET and PA6. Furthermore, the RMF values of PBT, PET and PA6 above Tmax are significant (18% at 480 °C for PET [38] 8% at 500 °C for PA6 [40]) but invariably lower than those of H-PAAs, which become negligible only above 600–650 °C.
Figure 4 shows the DSC thermograms of H-PAAs relating to the 2nd heating cycle at 10 °C min−1, and Figure S31 shows those pertaining to the cooling cycle. The onset melting temperatures, Tonset; the melting and crystallization temperatures, Tm and Tc; the melting and crystallization enthalpies, ΔHm and ΔHc; and the glass transition temperatures, Tg, are listed in Table 6. All H-PAAs, with the exception of B6-DE2, were semi-crystalline and provided evidence of melting (Figure 4c) and crystallization (Figure S31c). In particular, samples B12-PIP, B6-PIP, B12-DM2 and B6-DM6 showed bimodal melting traces. Quite surprisingly, B10-DM6 showed evidence of melting (Figure 4e) but not of extensive recrystallization (Figure S31e). Furthermore, both PIP-based samples exhibited particularly high Tm2 values: 196/216 and 223/236 °C for B12-PIP and B6-PIP, respectively (Table 6 and Figure 4b,d).
H-PAAs derived from both B12 (Figure 4a) and B6 (Figure 4c) showed the same ranking of Tm values based on the structure of the amine moiety: PIP > DM2 > DM6 > DE2. It should be remembered that B6-DE2 did not melt nor crystallize. Within the DM6 series, Tm2 values (100, 95, 90 and 84 °C for B12-DM6, B10-DM6, B8-DM6 e B6-DM6, respectively) were clearly dependent on the bis-acrylamide chain length and decreased by decreasing the number of the bis-acrylamide carbon atoms (Figure 4e). The ΔHm2 values also decreased by decreasing the number of carbon atoms in the series (63.3, 62.0, 57.1 and 51.1 Jg−1 for B12-DM6, B10-DM6, B8-DM6 e B6-DM6, respectively). The differences between the thermal data of B12-DM6 and bB12-DM6, and between those of B8-DM6 and bB8-DM6, were not relevant (Figure S32).
Regarding the cooling cycle, both B12-PIP and B6-PIP showed the highest crystallization temperatures, Tc, of the B12- and B6-series (179 °C for B12-PIP and 200 °C for B6-PIP), as already observed for Tm2 values. Furthermore, within the DM6-series, Tc showed almost the same trend observed for Tm2, with the exception of B12-DM6 and B12-DE2. The significant increase in the melting enthalpy of B12-DM6 compared with B8-DM6 can be explained by the greater mobility of the B12 chains that can arrange in larger crystalline domains.
The glass transition temperatures, Tg, of H-PAAs were between −10 and −23 °C, except for B12-PIP and B6-PIP, whose Tg values were 32 °C and 55 °C, respectively. Remarkably, the Tg of B12-DE2 was not detectable. Within the DM6 series, the Tg values decreased slightly as the bis-acrylamide chain length increased (−19, −19, −20, and −23 °C for B12-DM6, B10-DM6, B8-DM6 and B6-DM6, respectively). The Tg values of bB12-DM6 and bB8-DM6 were slightly higher than those of the corresponding samples obtained in solution. This is likely due to the presence, in the latter, of the residual impurities of benzyl alcohol.

3.5. Preliminary Evaluation of the Effect of Water Contact on the Macroscopic Properties of H-PAA Films

H-PAA films with an average thickness of 0.2 mm were prepared by compression molding. The specimens were visually evaluated for their flexibility and ability to withstand small stresses and then placed in contact with water to ascertain the effect of water on the observed properties (see Table 7). These tests provided the criteria for selecting B12-DM6 and B8-DM6 as the best H-PAA samples for studying the feasibility of the bulk polymerization process and further evaluating the wettability and tensile properties of the resulting bB12-DM6 and bB8-DM6 samples.

3.6. Ignitability Tests

The ignitability of H-PAAs was assessed by direct flame impingement for 10 s on powdered samples (snapshots reported in Figure 5). The samples did not ignite when the flame was applied and exhibited minimal weight loss (<5%). Their surface melted and decomposed, yellowing slightly, and produced carbonaceous crusts that protected the underlying powders, which remained white and apparently intact. This behavior testified the tendency of H-PAAs to intumesce upon heating and was in line with previous ignitability data obtained with hydrophilic PAAs [29,42]. It also demonstrated that inserting a large hydrophobic moiety in their repeating unit did not significantly affect their flame resistance. The inherent intumescent behavior of PAAs is a rarely seen feature in polymeric flame retardants. Similar behavior, in fact, has been observed only in DNA and in some proteins for which, however, industrial exploitation for this purpose is almost inconceivable [43,44,45].

3.7. Preliminary Evaluation of Tensile Properties of bB12-DM6 and bB8-DM6

The tensile properties of bB12-DM6 and bB8-DM6 were investigated on 0.1 mm thick dog bone shaped specimens following the ISO 37-2011 standard. The results are shown in Figure 6 and Table 8.
It is evident that bB12-DM6 and bB8-DM6 have a similar Young’s modulus. It should be noted that they have similar molecular weights, despite their degrees of polymerization being somewhat different. Furthermore, the samples did not undergo a visible yield before failure. It can also be observed that all tensile data, i.e., the strain at break, the stress at break and the maximum stress of the two samples, differed significantly. Not surprisingly, these values increased from bB8-DM6 to bB12-DM6, i.e., by increasing the length of the bis-acrylamide hydrocarbon chain. The greater maximum stress value of B12-DM6, compared with B8-DM6, is linked to the greater crystallinity of the first polymer, as also highlighted by the thermal data.

3.8. Wettability

The wettability of bB12-DM6 and bB8-DM6 was assessed by measuring the contact angle with water using the sessile drop method. Contact angles were measured both near the center and at the edge of the samples. Results are reported in Figure 7 and Table 9. It is evident that the wettability of bB12-DM6 was significantly lower than that of bB8-DM6, as expected. In fact, the proportion between the hydrophobic chains and the hydrophilic amide and amine groups of the former is higher.

4. Conclusions

The aim of this work was to prepare linear hydrophobic semi-crystalline PAAs with fair physical and mechanical properties using hydrophobic bis-acrylamides and bis-sec-amines as monomers. A small library of twelve linear H-PAAs was synthesized and characterized. A preliminary investigation into the relationship between structure and relevant physical properties allowed us to select a limited number of samples, investigated with regards to wettability and tensile properties.
H-PAAs were prepared by both solution and bulk processes. Initially, all the samples were prepared by a solution process, by analogy with the linear PAAs described so far in the literature, employing benzyl alcohol as the solvent. The samples selected for wettability and tensile tests, i.e., bB12-DM6 and bB8-DM6, were also prepared by a bulk process, never previously described for the synthesis of PAAs. The bulk process was carried out under a nitrogen atmosphere at a temperature well above the melting points of both the monomers and the resulting polymers and in the presence of a radical inhibitor. This process proved more effective as it led to samples with no need for further purification. The number of the average molecular weights of bB12-DM6 and bB8-DM6 did not differ significantly from those of the corresponding samples obtained from the solution process.
The H-PAAs obtained by the solution process were first screened for the molecular weight obtainable and, subsequently, physical properties including thermal properties, filmability, flammability, apparent strength and water resistance. Samples B12-DB2 and B6-DB2 were discarded due to their low molecular weight, as revealed by the significant presence of residual double bonds in their 1H-NMR spectra. Furthermore, they were sticky and apparently unable to crystallize. All remaining H-PAAs were semi-crystalline, with the sole exception of B6-DE2. The melting temperatures of the H-PAAs derived from the same amine, namely DM6, clearly increased by increasing the length of the bis-acrylamide moiety. Those of the H-PAAs derived from the same bis-acrylamide and different bis-amines also depended on the structure of the amine substituent. The order for H-PAAs-derived B12 and B6 was PIP >> DM2 > DM6 > DE2. B6-DE2 did not crystallize.
Overall, the thermal stability of H-PAAs was considerably higher, in terms of Tonset10% and Tmax, than those of the hydrophilic PAAs studied so far [29]. Furthermore, as hydrophilic PAAs, they were significantly more stable in air than in nitrogen, and they exhibited greater residue formation, which was not present in the TGA traces of many commercial polymers, including Nylons and PET. The residual mass fraction of H-PAAs in the air at 550 °C varied between 10 and 13%. The residual mass fractions at 400 °C made it possible to identify the correlations between thermal stability and the number of carbon atoms in the bis-acrylamide moiety. The influence of the amino moiety structure was not uniquely identified, except in the case of the H-PAAs derived from piperazine, which were the most thermally stable considering both Tonset10% and Tmax.
Ignitability tests proved that resistance to direct flame impingement was excellent in all cases. The samples melted but did not burn and partially decomposed on the surface, turning yellow. The interior remained apparently intact.
H-PAAs were completely insoluble in water. However, the films of half of them became brittle when in contact with water. The H-PAAs most resistant to contact with water were B12-DM6 and B8-DM6. Subsequently, they were synthesized in bulk and characterized by wettability and tensile tests. They showed a similar Young’s modulus (260 for B8-DM6 and 267 MPa for B12-DM6), while the maximum stress, stress at break and strain at break increased from B8-DM6 to B12-DM6, apparently depending on the number of methylene groups in the bis-acrylamide moieties.

Supplementary Materials

The following are available online at https://www.mdpi.com/article/10.3390/polym13071018/s1, Figures S1–S3: 1H-NMR spectra of bis-acrylamides with assignments. Figures S4–S16: 1H-NMR spectra of H-PAAs with assignments. Figures S17–S29: FT-IR/ATR spectra of H-PAAs with assignments. Figure S30: TGA curves of B12-DM6 derived from solution and bulk synthesis in nitrogen (a) and air (b). Figures S31–S44: DSC thermograms of H-PAAs.

Author Contributions

Conceptualization, P.F. and A.M.; methodology, all the Authors contributed equally; formal analysis, A.M. and J.A.; investigation, M.M. (Massimo Marcioni), A.M., M.M. (Mario Malinconico) and P.L.; data curation, M.M.; writing—original draft preparation, A.M., E.R. and P.F.; writing—review and editing, A.M. and J.A.; supervision, A.M., E.R. and P.F. All authors have read and agreed to the published version of the manuscript.

Funding

The research was funded by Università degli Studi di Milano, Piano di sostegno alla ricerca 2018–2019, Linea 2 PSR2018_DIP_005.

Institutional Review Board Statement

Not applicable.

Informed Consent Statement

Not applicable.

Data Availability Statement

Not applicable.

Acknowledgments

The authors thanks Salvatore Mallardo (IPCB) for the technical assistance.

Conflicts of Interest

The authors declare no conflict of interest.

References

  1. Ferruti, P. Polyamidoamines: Past, Present and Perspectives. J. Polym. Sci. Polym. Chem. 2013, 51, 2319–2353. [Google Scholar] [CrossRef]
  2. Ranucci, E.; Manfredi, A. Polyamidoamines: Versatile bioactive polymers with potential for biotechnological applications. Chem. Afr. 2019, 2, 167–193. [Google Scholar] [CrossRef]
  3. Mather, B.D.; Visvanathan, K.; Millerb, K.M.; Long, T.E. Michael addition reactions in macromolecular design for emerging technologies. Prog. Polym. Sci. 2006, 31, 487–531. [Google Scholar] [CrossRef]
  4. Ferruti, P.; Marchisio, M.A.; Duncan, R. Poly(amido-amine)s: Biomedical Applications. Macromol. Rapid Commun. 2002, 23, 332–355. [Google Scholar] [CrossRef]
  5. Ferruti, P.; Ranucci, E.; Bignotti, F.; Sartore, L.; Bianciardi, P.; Marchisio, M.A. Degradation Behaviour of Ionic Stepwise Polyaddition Polymers of Medical Interest. J. Biomater. Sci. Polym. Ed. 1995, 6, 833–844. [Google Scholar] [CrossRef]
  6. Arioli, M.; Manfredi, A.; Alongi, J.; Ferruti, P.; Ranucci, E. Highlight on the Mechanism of Linear Polyamidoamine Degradation in Water. Polymers 2020, 12, 1376. [Google Scholar] [CrossRef] [PubMed]
  7. Barbucci, R.; Casolaro, M.; Nocentini, M.; Corezzi, S.; Ferruti, P.; Barone, V. Acid-Base and Metal Ion Complex Formation Properties of Polymers Containing Amino Acid Residues. Macromolecules 1986, 19, 37–42. [Google Scholar] [CrossRef]
  8. Sartore, L.; Penco, M.; Della Sciucca, S.; Borsarini, G.; Ferrari, V. New carbon black composite vapor detectors based on multifunctional polymers. Sensors Actuat. B Chem. 2005, 111, 160–165. [Google Scholar] [CrossRef]
  9. Sartore, L.; Barbaglio, M.; Borgese, L.; Bontempi, E. Polymer-grafted QCM chemical sensor and application to heavy metal ions real time detection. Sensors Actuat. B Chem. 2011, 155, 538–544. [Google Scholar] [CrossRef]
  10. Sartore, L.; Barbaglio, M.; Penco, M.; Bergese, R.; Bontempi, E.; Colombi, P.; Depero, L.E. Polymer-coated quartz crystal microbalance chemical sensor for heavy cations in water. J. Nanosci. Nanotechnol. 2009, 9, 1164–1168. [Google Scholar] [CrossRef] [PubMed]
  11. Barbucci, R.; Magnani, A. Physiochemical characterization and coating of polyurethane with a new heparin-adsorbing material. Biomaterials 1989, 10, 429–432. [Google Scholar] [CrossRef]
  12. Barbucci, R.; Casolaro, M.; Magnani, A.; Roncolini, C. FTi.r. and potentiometric study of basic polymer behaviour in the free form, in different bulks, in both solid state and aqueous solution. Polymer 1991, 32, 897–903. [Google Scholar] [CrossRef]
  13. Barbucci, R.; Albanese, A.; Magnani, A.; Tempesti, F. Coating of commercially available materials with a new heparinizable material. J. Biomed. Mater. Res. 1991, 25, 1259–1274. [Google Scholar] [CrossRef]
  14. Caldwell, G.; Neuse, E.; Stephanou, A. Synthesis of water-soluble polyamidoamines for biomedical applications. II. Polymers possessing intrachain-type secondary amino groups suitable for side-chain attachment. J. Appl. Polym. Sci. 1993, 50, 393–401. [Google Scholar] [CrossRef]
  15. Caldwell, G.; Neuse, E.W.; van Rensburg, C.E.J. Cytotoxicity of Selected Water-Soluble Polymer–cis-Diaminedichloroplatinum (II) Conjugates Against the Human HeLa Cancer Cell Line. J. Inorg. Organomet. Polym. 1997, P7, 217–231. [Google Scholar] [CrossRef]
  16. Bencini, M.; Ranucci, E.; Ferruti, P.; Trotta, F.; Donalisio, M.; Cornaglia, M.; Lembo, D.; Cavalli, R. Preparation and in vitro evaluation of the antiviral activity of the Acyclovir complex of a β-cyclodextrin/poly(amidoamine) copolymer. J. Control. Release 2008, 126, 17–25. [Google Scholar] [CrossRef] [PubMed]
  17. Mauro, N.; Ferruti, P.; Ranucci, E.; Manfredi, A.; Berzi, A.; Clerici, M.; Cagno, V.; Lembo, D.; Palmioli, A.; Sattin, S. Linear biocompatible glyco-polyamidoamines as dual action mode virus infection inhibitors with potential as broad-spectrum microbicides for sexually transmitted diseases. Sci. Rep. 2016, 6, 33393. [Google Scholar] [CrossRef]
  18. Donalisio, M.; Quaranta, P.; Chiuppesi, F.; Pistello, M.; Cagno, V.; Cavalli, R.; Volante, M.; Bugatti, A.; Rusnati, M.; Ranucci, E.; et al. The AGMA1 poly(amidoamine) inhibits the infectivity of herpes simplex virus in cell lines, in human cervicovaginal histocultures, and in vaginally infected mice. Biomaterials 2016, 85, 40–53. [Google Scholar] [CrossRef] [PubMed]
  19. Elzes, M.R.; Akeroyd, N.; Engbersen, J.F.J.; Paulusse, J.M.J. Disulfide-functional poly(amido amine)s with tunable degradability for gene delivery. J. Control. Release 2016, 244, 357–365. [Google Scholar] [CrossRef]
  20. Lim, H.; Noh, J.; Kim, Y.; Kim, H.; Kim, J.; Khang, G.; Lee, D. Acid-Degradable Cationic Poly (ketal amidoamine) for Enhanced RNAInterference In Vitro and In Vivo. Biomacromolecules 2013, 14, 240–247. [Google Scholar] [CrossRef]
  21. Cavalli, R.; Primo, L.; Sessa, R.; Chiaverina, G.; di Blasio, L.; Alongi, J.; Manfredi, A.; Ranucci, E.; Ferruti, P. The AGMA1 polyamidoamine mediates the efficient delivery of siRNA. J. Drug Target. 2017, 25, 891–898. [Google Scholar] [CrossRef] [PubMed]
  22. Sun, Y.; Liu, H.; Xing, H.; Lang, L.; Cheng, L.; Yang, T.; Yang, L.; Ding, P. Bioreducible poly (amido amine) copolymers derived from histamine and agmatine for highly efficient gene delivery. Polym. Int. 2019, 68, 447–455. [Google Scholar] [CrossRef]
  23. Ranucci, E.; Bignotti, F.; Paderno, P.L.; Ferruti, P. Modification of albumins by grafting poly (amido amine) chains. Polymer 1995, 36, 2989–2994. [Google Scholar] [CrossRef]
  24. Magnaghi, V.; Conte, V.; Procacci, P.; Pivato, G.; Cortese, P.; Cavalli, E.; Pajardi, G.; Ranucci, E.; Fenili, F.; Manfredi, A.; et al. Biological performance of a novel biodegradable polyamidoamine hydrogel as guide for peripheral nerve regeneration. J. Biomed. Mater. Res. Part A 2011, 98 A, 19–30. [Google Scholar] [CrossRef]
  25. Dos Reis, G.; Fenili, F.; Gianfelice, A.; Bongiorno, G.; Marchesi, D.; Scopelliti, P.E.; Borgonovo, A.; Podestà, A.; Indrieri, M.; Ranucci, E.; et al. Direct microfabrication of topographical and chemical cues for the guided growth of neural cell networks on polyamidoamine hydrogels. Macromol. Biosci. 2010, 10, 842–852. [Google Scholar] [CrossRef] [PubMed]
  26. Martello, F.; Tocchio, A.; Tamplenizza, M.; Gerges, I.; Pistis, V.; Recenti, R.; Bortolin, M.; Del Fabbro, M.; Argentiere, S.; Milani, P.; et al. Poly (amido-amine)-based hydrogels with tailored mechanical properties and degradation rates for tissue engineering. Acta Biomater. 2014, 10, 1206–1215. [Google Scholar] [CrossRef] [PubMed]
  27. Mauro, N.; Chiellini, F.; Bartoli, C.; Gazzarri, M.; Laus, M.; Antonioli, D.; Griffiths, P.; Manfredi, A.; Ranucci, E.; Ferruti, P. RGD-mimic polyamidoamine–montmorillonite composites with tunable stiffness as scaffolds for bone tissue-engineering applications. J. Tissue Eng. Regen. Med. 2017, 11, 2164–2175. [Google Scholar] [CrossRef]
  28. Gualandi, C.; Bloise, N.; Mauro, N.; Ferruti, P.; Manfredi, A.; Sampaolesi, M.; Liguori, A.; Laurita, R.; Gherardi, M.; Colombo, V.; et al. Poly-l-Lactic Acid Nanofiber–Polyamidoamine Hydrogel Composites: Preparation, Properties, and Preliminary Evaluation as Scaffolds for Human Pluripotent Stem Cell Culturing. Macromol. Biosci. 2016, 1533–1544. [Google Scholar] [CrossRef] [PubMed]
  29. Manfredi, A.; Carosio, F.; Ferruti, P.; Ranucci, E.; Alongi, J. Linear polyamidoamines as novel biocompatible phosphorus-free surface-confined intumescent flame retardants for cotton fabrics. Polym. Degrad. Stabil. 2018, 151, 52–64. [Google Scholar] [CrossRef]
  30. Schotten, C. Ueber die Oxydation des Piperidins. Ber. Dtsch. Chem. Ges. 1884, 17, 2544. [Google Scholar] [CrossRef]
  31. Baumann, E. Ueber eine einfache Methode der Darstellung von Benzoësäureäthern. Ber. Dtsch. Chem. Ges. 1886, 19, 3218. [Google Scholar] [CrossRef]
  32. Vogel, A.I. Practical Organic Chemistry, 3rd ed.; Longman Group Ltd.: London, UK, 1957; pp. 582–584. [Google Scholar]
  33. Fulmer, G.R.; Miller, A.J.M.; Sherden, N.H.; Gottlieb, H.E.; Nudelman, A.; Stoltz, B.M.; Bercaw, J.E.; Goldberg, K.I. NMR Chemical Shifts of Trace Impurities: Common Laboratory Solvents, Organics, and Gases in Deuterated Solvents Relevant to the Organometallic Chemist. Organometallics 2010, 29, 2176–2179. [Google Scholar] [CrossRef]
  34. Babij, N.R.; McCusker, E.O.; Whiteker, G.T.; Canturk, B.; Choy, N.; Creemer, L.C.; De Amicis, C.V.; Hewlett, N.M.; Johnson, P.L.; Knobelsdorf, J.A.; et al. NMR Chemical Shifts of Trace Impurities: Industrially Preferred Solvents Used in Process and Green Chemistry. Org. Process. Res. Dev. 2016, 20, 661–667. [Google Scholar] [CrossRef]
  35. Aboulkas, A.; El Harfi, K.; El Bouadili, A. Thermal degradation behaviors of polyethylene and polypropylene. Part I: Pyrolysis kinetics and mechanisms. Energy Convers. Manag. 2010, 51, 1363–1369. [Google Scholar] [CrossRef]
  36. Bolbukh, Y.; Kuzema, P.; Tertykh, V.; Laguta, I. Thermal degradation of polyethylene containing antioxidant and hydrophilic/hydrophobic silica. J. Therm. Anal. Calorim. 2008, 94, 727–736. [Google Scholar] [CrossRef]
  37. Matzen, M.; Kandola, B.; Huth, C.; Schartel, B. Influence of Flame Retardants on the Melt Dripping Behaviour of Thermoplastic Polymers. Materials 2015, 8, 5621–5646. [Google Scholar] [CrossRef] [PubMed]
  38. Gorrasi, G.; Milone, C.; Piperopoulos, E.; Pantani, R. Preparation, processing and analysis of physical properties of calciumferrite-CNTs/PET nano-composite. Compos. Part B 2015, 81, 44–52. [Google Scholar] [CrossRef]
  39. Holland, B.J.; Hay, J.N. The thermal degradation of PET and analogous polyesters measured by thermal analysis-Fourier transform infrared spectroscopy. Polymer 2002, 43, 1835–1847. [Google Scholar] [CrossRef]
  40. Zhao, M.; Yi, D.; Camino, G.; Frache, A.; Yang, R. Interdigitated crystalline MMT-MCA in polyamide 6. RSC Adv. 2017, 7, 861–869. [Google Scholar] [CrossRef]
  41. Fina, A.; Camino, G. Ignition mechanisms in polymers and polymer nanocomposites. Polym. Adv. Technol. 2011, 22, 1147–1155. [Google Scholar] [CrossRef]
  42. Manfredi, A.; Carosio, F.; Ferruti, P.; Alongi, J.; Ranucci, E. Disulfide-containing polyamidoamines with remarkable flame retardant activity for cotton fabrics. Polym. Degrad. Stab. 2018, 156, 1–13. [Google Scholar] [CrossRef]
  43. Alongi, J.; Cuttica, F.; Di Blasio, A.; Carosio, F.; Malucelli, G. Intumescent features of nucleic acids and proteins. Termochim. Acta 2014, 591, 31–39. [Google Scholar] [CrossRef]
  44. Costes, L.; Laoutid, F.; Brohez, S.; Dubois, P. Bio-based flame retardants: When nature meets fire protection. Mater. Sci. Eng. R 2017, 117, 1–25. [Google Scholar] [CrossRef]
  45. Salmeia, K.A.; Gaan, S.; Malucelli, G. Recent Advances for Flame Retardancy of Textiles Based on Phosphorus Chemistry. Polymers 2016, 8, 319. [Google Scholar] [CrossRef] [PubMed]
Scheme 1. Synthesis of the bis-acrylamides used in H-PAA syntheses.
Scheme 1. Synthesis of the bis-acrylamides used in H-PAA syntheses.
Polymers 13 01018 sch001
Figure 1. 1H-NMR spectrum of bis-acrylamide B12 obtained in CD3OD using a 400 MHz Avance Brüker spectrometer. Water assignment was in agreement with the literature [33,34].
Figure 1. 1H-NMR spectrum of bis-acrylamide B12 obtained in CD3OD using a 400 MHz Avance Brüker spectrometer. Water assignment was in agreement with the literature [33,34].
Polymers 13 01018 g001
Scheme 2. Synthesis of H-PAAs.
Scheme 2. Synthesis of H-PAAs.
Polymers 13 01018 sch002
Figure 2. 1H-NMR spectrum of H-PAA B12-DM2 obtained in CDCl3 using a 400 MHz Avance Brüker spectrometer.
Figure 2. 1H-NMR spectrum of H-PAA B12-DM2 obtained in CDCl3 using a 400 MHz Avance Brüker spectrometer.
Polymers 13 01018 g002
Figure 3. TGA thermograms of H-PAAs: panels (a,c,e) in nitrogen; panels (b,d,f) in air.
Figure 3. TGA thermograms of H-PAAs: panels (a,c,e) in nitrogen; panels (b,d,f) in air.
Polymers 13 01018 g003
Figure 4. Differential scanning calorimetric (DSC) thermograms pertaining to the 2nd heating cycle at 10 °C min−1 of: (a) B12-DM2, B12-DM6 and B12-DE2; (b) B12-PIP; (c) B6-DM2, B6-DM6 and B6-DE2; (d) B6-PIP; (e) B6-DM6, B8-DM6, B10-DM6 and B12-DM6.
Figure 4. Differential scanning calorimetric (DSC) thermograms pertaining to the 2nd heating cycle at 10 °C min−1 of: (a) B12-DM2, B12-DM6 and B12-DE2; (b) B12-PIP; (c) B6-DM2, B6-DM6 and B6-DE2; (d) B6-PIP; (e) B6-DM6, B8-DM6, B10-DM6 and B12-DM6.
Polymers 13 01018 g004
Figure 5. Snapshot of the results of ignitability tests carried out on H-PAA powders.
Figure 5. Snapshot of the results of ignitability tests carried out on H-PAA powders.
Polymers 13 01018 g005
Figure 6. Graphical representation of bB12-DM6 and bB8-DM6 tensile properties.
Figure 6. Graphical representation of bB12-DM6 and bB8-DM6 tensile properties.
Polymers 13 01018 g006
Figure 7. Contact angle measurements on bB12-DM6 (upper row) and bB8-DM6 (lower row) films: contact point close to the border (left panels); contact point near the center of the specimen (right panels).
Figure 7. Contact angle measurements on bB12-DM6 (upper row) and bB8-DM6 (lower row) films: contact point close to the border (left panels); contact point near the center of the specimen (right panels).
Polymers 13 01018 g007
Table 1. Amounts of reagents used in the synthesis of bis-acrylamides (a).
Table 1. Amounts of reagents used in the synthesis of bis-acrylamides (a).
Polymers 13 01018 i001
CodeN (b)Amine (c)
(g)
Yield
(g)
Yield
(%)
B121031.027.760.0
B10826.424.057.0
B8622.126.570.0
B6417.820.561.0
(a) In all cases, the amount of acryloyl chloride was 29.9 g (330 mmol). (b) Number of CH2 groups reported in parentheses; (c) 150 mmol.
Table 2. Amounts of reagents used in the synthesis of H-PAAs by solution (a,b) and bulk processes. (b,c)
Table 2. Amounts of reagents used in the synthesis of H-PAAs by solution (a,b) and bulk processes. (b,c)
Sample Code (d)Bis-Acrylamide
(g)
Bis-Amine
(g)
Benzyl
Alcohol
(mL)
Time
(h)
Yield
[g, (%)]
M ¯ n
B12-DM215.44.557.04817.7 (89)9700
B12-DM615.47.465.04821.3 (93)>10,000
B12-DE215.45.961.04818.7 (88)6000
B12-DB215.412.483.09619.5 (70)<3000
B12-PIP15.44.459.04819.6 (99)6400
B10-DM614.07.461.04820.4 (95)6000
B8-DM612.67.460.04818.5 (92)6400
B6-DM211.24.546.04813.3 (85)>10,000
B6-DM611.27.455.04815.5 (83)>10,000
B6-DE211.25.951.04811.3 (66)6000
B6-DB211.212.469.096n.d. (e)<3000
B6-PIP11.24.445.048(98)>10,000
bB12-DM6 (f)15.47.4-3(~100)7500
bB8-DM6 (f)12.67.4-3(~100)6400
(a) Temperature = 60 °C. (b) Monomer amounts: 50 mmol. (c) Temperature = 70–140 °C. (d) B12: 1,12-dodecamethylene-bis-acrylamide; B10: 1,10-decamethylene-bis-acrylamide; B8: 1,8-octamethylene-bis-acrylamide; B6: 1,6-hexamethylene-bis-acrylamide; DM2: N,N’-dimethylethylenediamine; DM6: N,N’-dimethyl-1,6-hexanediamine; DE2: N,N’-diethylethylenediamine; DB2: N,N’-dibenzylethylenediamine; PIP: piperazine. (e) n.d.: not determined. (f) Sample obtained by the bulk process.
Table 3. Structure of H-PAAs.
Table 3. Structure of H-PAAs.
Polymer CodeStructure of the Repeat Unit
B12-DM2Polymers 13 01018 i002
B12-DE2Polymers 13 01018 i003
B12-DB2Polymers 13 01018 i004
B12-DM6Polymers 13 01018 i005
B12-PIPPolymers 13 01018 i006
B10-DM6Polymers 13 01018 i007
B8-DM6Polymers 13 01018 i008
B6-DM2Polymers 13 01018 i009
B6-DE2Polymers 13 01018 i010
B6-DB2Polymers 13 01018 i011
B6-DM6Polymers 13 01018 i012
B6-PIPPolymers 13 01018 i013
Table 4. Solubility of H-PAAs (a).
Table 4. Solubility of H-PAAs (a).
B12-DM2B12-DM6B12-DE2B12-DB2B12-PIPB10-DM6B8-DM6B6-DM2B6-DM6B6-DE2B6-DB2B6-PIP
Methanoliishshishshshshshshi
Ethanolshshshshishshshshshshi
Isopropanolshshshshishshshshshshi
Butanolshshshshshshshshshshshi
Benzyl alcoholshsssshshshshsSssh
Acetoneiiiiiiiiiiii
Dimethyl sulfoxideiiiiiiiiiiii
Diisopropyl etheriiiiiiiiiiii
Diethyl etheriiiiiiiiiiii
Chloroformssssissssssi
Dichloromethaneisssissssssi
Acetic acid/
water 1:2
iiiisiiiiiis
Wateriiiiiiiiiiii
(a) i: insoluble; s: soluble; sh: soluble at boiling point.
Table 5. Thermal data collected by thermogravimetric analyses (TGA).
Table 5. Thermal data collected by thermogravimetric analyses (TGA).
PolymerNitrogenAir
Tonset10% (a)
(°C)
Tmax1 (b)
(°C)
Tmax2
(°C)
RMF400 (c)
(%)
Tonset10%
(°C)
Tmax1
(°C)
Tmax2
(°C)
Tmax3
(°C)
RMF400
(%)
RMF550 (d)
(%)
B12-DM2281330460492853054626106814
B12-DE2265280462552682904645756311
B12-DM6270323459432692994656106113
B12-PIP315347458462973154605856922
B10-DM6273320456392702924656205712
B8-DM627832045233278300442/4606105211
B6-DM2278325445422753104485815516
B6-DE2265304445392683024475805012
B6-DM6266316440232663054505874310
B6-PIP286330438342823244465754311
bB12-DM6 (e)271318457412813004646176113
bB8-DM6 (e)27932245034277300441/4626125310
(a) Tonset10%: onset decomposition temperature at 10% weight loss; (b) Tmax: temperature at maximum weight loss rate; (c) RMF400 residual mass fractions measured at 400 °C; (d) RMF550 residual mass fractions measured at 550 °C; (e) sample produced by bulk polymerization process. RMF550 in air is negligible for all samples.
Table 6. Thermal data collected by DSC.
Table 6. Thermal data collected by DSC.
Polymer1st Heating CycleCooling Cycle2nd Heating Cycle
Tonset,m1 (a)
(°C)
Tm1 (b)
(°C)
ΔHm1 (c)
(Jg−1)
Tonset,cr (d)
(°C)
Tcr (e)
(°C)
ΔHcr (f)
(Jg−1)
Tonset,m2 (g)
(°C)
Tm2 (h)
(°C)
ΔHm2 (i)
(Jg−1)
Tg (l)
(°C)
B12-DM27083−23.4979149.3116123−76.6−10
B12-DM6---716158.695100−63.3−19
B12-DE2---807482.38395−95.5n.d. (m)
B12-PIP188195−51.318117948.5198196/216−18.3+32
B10-DM6---53443.28895−62.0−19
B8-DM6-- 534654.48690−57.1−20
B6-DM2---787253.6103111−54.5−13
B6-DM67684−37.1555048.18984−51.1−23
B6-DE2----------
B6-PIP216222−13.220520053.4228223/236−24.2+55
bB12-DM6---686234.698105−72.2−10
bB8-DM6 ---635753.093100−50.8−16
1st Heating cycle: (a) Tonset, m1: the onset temperature, the intersection of the tangent of the melting peak with the extrapolated baseline; (b) Tm1: melting temperature; (c) ΔHm1: enthalpy of melting. Cooling cycle: (d) Tonset, cr: the onset temperature defined as the intersection of the tangent of the crystallization peak with the extrapolated baseline; (e) Tcr: crystallization temperature; (f) ΔHcr: enthalpy of crystallization. 2nd Heating cycle: (g) Tonset, m2: the onset temperature defined as the intersection of the tangent of the melting peak with the extrapolated baseline; (h) Tm2: melting temperature; (i) ΔHm2: enthalpy of melting; (l) Tg: glass transition temperature; (m) n.d.: not detected.
Table 7. Preliminary evaluation of the effect of water contact on the macroscopic properties of H-PAA films (~20 °C).
Table 7. Preliminary evaluation of the effect of water contact on the macroscopic properties of H-PAA films (~20 °C).
PolymerApparent
Flexibility
Resistance to HandlingResistance after Contact with Water
B12-DM2++-
B12-DM6+++
B12-DE2++-
B12-PIP---
B10-DM6+++
B8-DM6+++
B6-DM2++-
B6- DM6+++
B6-DE2++-
B6-PIP--+
Table 8. Tensile data of bB8-DM6 and bB12-DM6.
Table 8. Tensile data of bB8-DM6 and bB12-DM6.
SampleThickness (mm)Young Modulus (MPa)Stress Max (a) (MPa)Stress at Break (MPa)Strain at Break (%)
bB8-DM60.10 ± 0.02260 ± 243.9 ± 0.22.1 ± 0.51.7 ± 0.2
bB12-DM60.12 ± 0.02267 ± 2310.0 ± 0.35.9 ± 1.96.9 ± 0.3
(a) Maximal value of the stress-strain curve.
Table 9. Wettability of H-PAAs.
Table 9. Wettability of H-PAAs.
Polymer SamplePlaceContact Angle (deg)Wetting Tension (dy/cm)Base (mm)Base Area (mm2)Sessile Volume (μL)
bB8-DM6Border39.956.07.644.832.0
bB8-DM6Center40.355.77.340.928.4
bB12-DM6Border60.535.96.128.828.3
bB12-DM6Center54.242.76.733.931.0
Publisher’s Note: MDPI stays neutral with regard to jurisdictional claims in published maps and institutional affiliations.

Share and Cite

MDPI and ACS Style

Marcioni, M.; Alongi, J.; Ranucci, E.; Malinconico, M.; Laurienzo, P.; Ferruti, P.; Manfredi, A. Semi-Crystalline Hydrophobic Polyamidoamines: A New Family of Technological Materials? Polymers 2021, 13, 1018. https://doi.org/10.3390/polym13071018

AMA Style

Marcioni M, Alongi J, Ranucci E, Malinconico M, Laurienzo P, Ferruti P, Manfredi A. Semi-Crystalline Hydrophobic Polyamidoamines: A New Family of Technological Materials? Polymers. 2021; 13(7):1018. https://doi.org/10.3390/polym13071018

Chicago/Turabian Style

Marcioni, Massimo, Jenny Alongi, Elisabetta Ranucci, Mario Malinconico, Paola Laurienzo, Paolo Ferruti, and Amedea Manfredi. 2021. "Semi-Crystalline Hydrophobic Polyamidoamines: A New Family of Technological Materials?" Polymers 13, no. 7: 1018. https://doi.org/10.3390/polym13071018

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.

Article Metrics

Back to TopTop