The Effect of Titanium Tetra-Butoxide Catalyst on the Olefin Polymerization
 
 
Font Type:
Arial Georgia Verdana
Font Size:
Aa Aa Aa
Line Spacing:
Column Width:
Background:
Article

Novel Chemical Architectures Based on Beta-Cyclodextrin Derivatives Covalently Attached on Polymer Spheres

1
Faculty of Chemistry, Alexandru Ioan Cuza University of Iasi, 11 Carol 1st Bvd, 700506 Iasi, Romania
2
Institute of Interdisciplinary Research—CERNESIM Centre, Alexandru Ioan Cuza University of Iasi, 11 Carol I, 700506 Iasi, Romania
3
Faculty of Applied Chemistry and Materials Science, University Politehnica of Bucharest, 1-7 Gh. Polizu Street, 011061 Bucharest, Romania
4
National Research and Development Institute for Chemistry and Petrochemistry—ICECHIM, 202 Splaiul Independenţei, 060021 Bucharest, Romania
5
Advanced Polymer Materials Group, University Politehnica of Bucharest, Gh. Polizu Street, 011061 Bucharest, Romania
*
Author to whom correspondence should be addressed.
Polymers 2021, 13(14), 2338; https://doi.org/10.3390/polym13142338
Submission received: 18 June 2021 / Revised: 12 July 2021 / Accepted: 14 July 2021 / Published: 16 July 2021
(This article belongs to the Special Issue Polymers Synthesis and Characterization)

Abstract

:
This study presents the synthesis and characterization of polymer derivatives of beta-cyclodextrin (BCD), obtained by chemical grafting onto spherical polymer particles (200 nm) presenting oxirane functional groups at their surface. The polymer spheres were synthesized by emulsion polymerization of styrene (ST) and hydroxyethyl methacrylate (HEMA), followed by the grafting on the surface of glycidyl methacrylate (GMA) by seeded emulsion polymerization. The BCD-polymer derivatives were obtained using two BCD derivatives with hydroxylic (BCD-OH) and amino groups (BCD-NH2). The degree of polymer covalent functionalization using the BCD-OH and BCD-NH2 derivatives were determined to be 4.27 and 19.19 weight %, respectively. The adsorption properties of the materials were evaluated using bisphenol A as a target molecule. The best fit for the adsorption kinetics was Lagergren’s model (both for Qe value and for R2) together with Weber’s intraparticle diffusion model in the case of ST-HEMA-GMA-BCD-NH2. The isothermal adsorption evaluation indicated that both systems follow a Langmuir type behavior and afforded a Qmax value of 148.37 mg g−1 and 37.09 mg g−1 for ST-HEMA-GMA-BCD-NH2 and ST-HEMA-GMA-BCD-OH, respectively. The BCD-modified polymers display a degradation temperature of over 400 °C which can be attributed to the existence of hydrogen bonds and BCD thermal degradation pathway in the presence of the polymers.

Graphical Abstract

1. Introduction

Bisphenol A (BPA) is one of the most abundant chemical synthetic additives produced for the manufacturing of epoxy resins, polysulfones, unsaturated polyesters, polyacrylate resins polycarbonate plastics, and rubber [1,2]. Human exposure to BPA [3,4] or its bisphenol-based substitutes [5] exhibited cytotoxicity, neurotoxicity, endocrine-disrupting effects, reproductive toxicity, uterine cancer, and interference of cellular pathways, capable of mimicking some of the hormones of the human body [1,3,4,5]. A recent study [6] revealed that the estimated intake of BPA is 30.76 ng/kg per body weight per day, as this compound enters in various environmental media (air, soil, aquatic systems) and the food chain due to improper recycling procedures [1,7]. This value, although in some countries did not exceed the maximum acceptable values for daily intake, is all the more worrying as the first six countries with the highest values belong to the European Union [6]. Thus, it is of tremendous importance on the one hand to develop efficient decontamination procedures and on the other hand to impose stricter laws regarding plastic manufacturing or recycling.
Different methods for BPA removal were directed to biological treatment, membrane adsorption processes, or advanced oxidation [1]. The biological treatment involves the degradation of BPA by immobilization of enzymes such as oxidoreductase or polyphenol oxidases [8] that are capable of oxidizing organic pollutants, such as phenols, organic dyes, or drugs. Advanced oxidation is a method that removes BPA by the generation of highly reactive radicals or the application of photocatalytic treatment to break down the molecules of BPA into less harmful compounds from water, sediment, and soil [1,9,10,11]. The membrane adsorption technology is based on the selective adsorption capacity of different membranes of targeted pollutants (by chemical or physical interaction) and is sometimes preferred for BPA removal since it does not generate new harmful by-products [12,13].
The drawbacks of these methods are not only related to the potential of generating harmful by-products but also to the difficulty of controlling the necessary parameters for efficient removal of BPA (such as pH and temperature in the case of enzymes or photocatalytic removal) and laborious/expensive synthesis methods for adsorption membranes [2].
Cyclodextrins (CDs) are a class of three-dimensional (3D) cyclic oligosaccharides composed of d-glucose units linked together by α-1,4-glucosidic bonds with hydrophilic surface and hydrophobic internal hollow [14,15]. The amphiphilic, biodegradable, and non-hazardous properties of such compounds, as well as the possibility to design new cyclodextrin derivatives, has led to a wide range of applications for drug delivery systems, antiviral therapy, cosmetics, agriculture, enzymology, catalysis, enantiomers separation, and environmental protection, in which it has been shown they can be excellent candidates for decontamination of aqueous media, air or soil [15,16,17,18,19].
As environmental issues are becoming more important, intense research interest has been dedicated to the removal of pollutants from water using different cyclodextrins-polymer systems that are tailored to eliminate organic or inorganic pollutants based on the adsorption process of the targeted molecule [20,21,22]. Based on the 3D spatial structure of CDs and on the hydrophilic/hydrophobic building, the enhanced removal of pollutants is based on guest-host interactions between the cyclodextrin derivative and the targeted pollutant. The additional presence of polymer chains can improve the adsorption capacity of the contaminating agent depending on their chemical structure or morphology, since polymer adsorbents can include polymers with a spherical shape, intrinsic porosity, metal/covalent-organic frameworks, as well as hyper-crosslinked polymers [23,24,25].
Thus, literature data is abundant in different synthesis approaches that have the same goal, to improve the adsorption efficiency of the cyclodextrins-polymers (CDP) systems for wastewater decontamination. For example, beta-cyclodextrin (BCD) was reacted with epichlorohydrin (EPI) and further with trimesoyl chloride to obtain a CDP system that was further embedded by interfacial cross-linking into a nylon microfiltration membrane to create a porous structure with enhanced adsorption capacities of water contaminants [26]. The adsorption efficiency capacity of modified BCD is amazing considering that structurally different contaminants like BPA, methylene blue, and copper can be adsorbed simultaneously by using citric acid-crosslinked-BCD polymers [27]. Recent approaches demonstrated that BCD-based polymers obtained by crosslinking with EPI can be used in municipal wastewater treatment pilot plants to remove several micropollutants, including BPA, with over 80% efficiency [28]. Also, the BCDP adsorption capacities were improved by the presence of nano-adsorbents such as Fe3O4, SiO2, silver nanoparticles, or carbon nanotubes due to their high specific surface area and absence of internal diffusion resistance that enhances the kinetics for the adsorption processes of different contaminating agents such as BPA, organophoshorous insecticides, or p-nitrophenol from water [9,20,29].
Thus, in this work, novel BCD modified polymer particles with spherical morphology were synthesized for a possible decontamination process of wastewater. Utilizing the oxirane functional groups present at the surface of polymer particles, two types of BCD derivatives (with hydroxylic (BCD-OH) and amino groups (BCD-NH2)—Scheme 1) were chemically grafted to the polymer colloids (Scheme 2). The materials designed aimed to improve the interaction between the polymeric adsorbent, pollutant, and the contaminated media. One of the main goals of this study was to determine the linking capacities of the BCD to the polymer, as well as the maximum complexation capacity of the BCD-modified polymers toward a targeted molecule. Thus, BPA was selected as a model molecule to investigate the adsorption kinetics, complexation mechanism, and isotherms.

2. Materials and Methods

2.1. Materials

Styrene (ST) (Sigma-Aldrich, St. Louis, MO, USA) has been purified through vacuum distillation. 2-Hydroxyethyl methacrylate (HEMA) (Sigma-Aldrich, St. Louis, MO, USA) and glycidyl methacrylate (GMA) (Merck, Darmstadt, Germany) have been purified by passing over short columns of activated basic alumina. Potassium persulfate (K2S2O8) (KPS) (Merck, Darmstadt, Germany) has been recrystallized from an ethanol/water mixture and then vacuum-dried. β-cyclodextrin (BCD-OH) (≥95.0%, Wacker Chemie, Munich, Germany) was vacuum-dried before use for 24 h. p-Toluene sulfonyl chloride (Ts-Cl) (reagent grade, ≥98%, Merck, Darmstadt, Germany), sodium hydroxide (reagent grade, ≥98%, pellets (anhydrous), (Sigma-Aldrich, St. Louis, MO, USA), 1,4-Diaminobutane (99%, Sigma-Aldrich, St. Louis, MO, USA), acetone (for analysis, >99%, Chemical Company Iasi), dimethyl sulfoxide (DMSO) (Aldrich-anhydrous, Darmstadt, Germany), pyridine (Aldrich, Darmstadt, Germany), glucose (Aldrich anhydrous, Darmstadt, Germany), phenol (Merck, Darmstadt, Germany), sulfuric acid (Sigma-Aldrich, St. Louis, MO, USA), bisphenol A (Merck, Darmstadt, Germany), ethanol (Chimopar, Bucuresti, România) were used as received.

2.2. Methods

2.2.1. ST-HEMA Emulsion Polymerization

A mixture of ST (1.3 mL), respectively, HEMA (0.3 mL) and KPS (25 mg) was added to distilled water (20 mL). The mixture was purged with nitrogen and then maintained for 8 h at 75 °C under continuous stirring. The final dispersion was dialyzed in distilled water for 7 days, using cellulose dialysis membranes (molecular weight cut-off: 12,000–14,000), to remove the unreacted monomers and initiator.

2.2.2. Seeded Emulsion Polymerization of GMA (ST-HEMA-GMA)

To the dialyzed emulsion presented previously was added 0.3 mL GMA and KPS (25 mg). The mixture was purged with nitrogen and then maintained for 8 h at 75 °C under continuous stirring. The final dispersion was dialyzed in distilled water for 7 days, using cellulose dialysis membranes (molecular weight cut-off: 12,000–14,000), to remove the unreacted monomers and initiator.

2.2.3. Synthesis of Diamino Butane Monosubstituted BCD (BCD-NH2)

The Ts-BCD was synthesized by a method similar to that reported by Brady et al. [30] (For the NMR spectra and Maldi see Supporting info Figures S1 and S2). The procedure for obtaining BCD-NH2 was as follows: 5.5 g Ts-BCD (4.266 mmol) were dissolved in 166 mL of 1,4-diaminobutane (DAB), slowly warmed up to 70 °C, and kept at this temperature for 24 h. At the end of reaction time, the solvent was vacuum distilled and the solid resulted was dissolved in a minimum amount of water. This syrup was added dropwise into 150–200 mL of acetone and precipitates a white solid. At least two acetone precipitations are needed to obtain a white powder solid, otherwise the product seems oily. The final product was obtained by drying the sample in a vacuum oven at 40 °C for 2 days with a 54% yield. 1H-NMR (DMSO-d6, 500 MHz): δ 1.405 (m, H-8, H-9), 2.5–2.562 (s, NH2, NH, DMSO), 2.688 (m, H-7), 2.882–2.860 (m, H-10), 3.346–3.304 (m, H-2, H-4), 3.627–3.551 (m, H-3, H-5, H-6), 4.474 (s, 6-OH), 4.823 (s, H-1), 5.736 (br, 2-OH and 3-OH) and 13C NMR (DMSO-d6, 125 MHz): δ 26.94 (C-9), 29.33 (C-8), 40.69 (C-10), 49.05 (C-7), 49.40 (C-6), 59.93 (C-6*), 72.05 (C-5), 72.43 (C-2), 73.07 (C-3), 81.55 (C-4), 101.96 (C-1). (see Supplementary information Figures S3–S6)).
MALDI: calc. for C46H80N2O34, M is 1204.45 Da (monoisotopic mass); the simple [M]+ or [M+H]+ were not identified but the mass 1215 corresponds to a complex adduct [2M+Na]2+.

2.2.4. The Reaction of BCD-OH with ST-HEMA-GMA

The ST-HEMA-GMA emulsion was dried in an oven at 70 °C on a glass plate. A solid powder was obtained after the water evaporation. 0.5 g ST-HEMA-GMA powder was dispersed in 10 mL DMSO and heated to 80 °C. After 30 min, 0.6 g BCD-OH was added to the mixture together with 0.01 mL pyridine, as catalysis. The reaction was kept to the temperature for 12 h and precipitated into hot water. The obtained white powder was filtered and dried in the oven.

2.2.5. The Reaction of BCD-NH2 with ST-HEMA-GMA

0.5 g ST-HEMA-GMA powder was dispersed in 10 mL DMSO and heated to 80 °C. After 30 min, 0.7 g BCD-NH2 was added to the mixture together with 0.01 mL pyridine, as catalysis. The reaction was kept to the temperature for 12 h and precipitated into hot water. The obtained white powder was filtered and dried in the oven.

2.3. Characterization

The morphology of the polymer nanoparticles was evaluated using transmission electron microscopy (TEM) (Tecnai G2 F20 TWIN Cryo-TEM, FEI Company), at 300 kV acceleration voltage, at a 1 Å resolution.
FTIR spectra were recorded on a Bruker VERTEX 70 spectrometer using 32 scans with a resolution of 4 cm−1 in 4000–600 cm−1 region. The samples were analyzed using the attenuated total reflection (ATR) technique.
The UV-Vis spectra were recorded using a V-550 Able Jasco spectrophotometer, using a bandwidth of 1 nm, and a scanning speed of 1000 nm min−1. The BCD content was quantified by determining the reducing sugars of the polymer using concentrated H2SO4 acidolysis and phenol colorimetric analysis [31]. The procedure employed for the determination of BCD content and the calibration curve are presented in the Supporting Info.
The thermogravimetric analyses (TGA) were performed using a Netzsch TG 209 F3 Tarsus equipment considering the next parameters: nitrogen atmosphere flow rate 20 mL min−1; samples mass: ∼3 mg; temperature range: room temperature −700 °C; heating rate: 10 °C min−1 in an alumina crucible.
NMR experiments were carried out on Bruker Avance III 500, 1H NMR spectra were recorded at 500 MHz using the solvent peaks as internal references and 13C NMR spectra were recorded at 125 MHz. All NMR experiments were conducted according to the literature, and they can be found in the supplementary material.
Matrix-assisted laser desorption ionization time of flight (MALDI-TOF) mass spectrometry experiments were carried out on Shimadzu AXIMA Performance, operated in high-resolution reflectron mode using α-Cyano-4-hydroxycinnamic acid as matrix.
The fluorescence spectra have been registered using a FP-6500 Able Jasco spectrofluorometer.

3. Results and Discussion

The first stage of our study consisted in the synthesis of polymeric particles presenting the capacity for the chemical attachment of BCD derivatives (BCD-OH and BCD-NH2, Scheme 1). The spherical shape was selected due to its high specific surface and high surface-to-volume ratio. The presence of an oxirane functional group at the surface of the polymer particles also permits the grafting of both beta-cyclodextrin derivatives (BCD-OH and BCD-NH2). Therefore, the synthesis strategy involved the emulsion polymerization of ST-HEMA system [32], followed by the seeded polymerization of GMA on the surface of the polymer particles [33]. As a result, an oxirane functional group capable of reacting with both hydroxyl and amino functional groups will be present on the surface of the polymer particles after the seeded polymerization. Figure 1 presents TEM images of the polymer particles at different stages during the synthesis route: ST-HEMA (after the emulsion polymerization), ST-HEMA-GMA (after the seeded polymerization), and ST-HEMA-GMA-BCD-NH2 (after BCD-NH2 grafting to the polymeric particle).
From the analysis of Figure 1, it can be observed that the ST-HEMA polymer particles are around 200 nm with a monodisperse size distribution. The average particle size and the size distribution are increased after the GMA seeded polymerization. Thus, the average particle size increases to around 220–230 nm, and a core-shell structuring can be noticed (inset detail Figure 1b). In the case of BCD-NH2 and BCD-OH grafting on the surface of the polymer particles, aggregates with an average dimension of 20 nm [34] can be observed deposited on the polymer particles after the seeded polymerization (darker spheres around the ST-HEMA-GMA Figure 1c,d).
To sustain the chemical grafting of the BCD derivative through the oxirane group reaction, the materials were analyzed by FT-IR spectroscopy (Figure 2). Thus, the specific vibration of oxirane 907 cm−1 decreased while the intensity of the signal at 3420 cm−1, specific for -OH vibration increased. Moreover, the appearance of C-O-C vibration signal at 1033 cm−1 and 3266 cm−1 signal specific for NH vibration confirm the chemical attachment of the BCD derivatives to the polymeric particles. The signal at 1026 cm−1 specific for the vibration of primary alcohol functional groups can also be identified in the ST-HEMA-GMA-BCD-OH and ST-HEMA-GMA-BCD-NH2 samples. In addition, the C−N bond that is formed during BCD-NH2 grafting to the polymer particles can be highlighted in the BCD-NH2 and ST-HEMA-GMA-BCD-NH2 samples at 1143 cm−1.
After the BCD attachment to the surface of the polymer particles, the degree of grafting was determined by NMR, TGA, and UV-Vis spectroscopy (see Supporting info Figure S7—calibration curve and determination method). Thus, BCD-OH content was determined at 4.27%, while in the case of BCD-NH2 the content was significantly higher at 19.19%. The difference in BCD content in the final materials can be explained by the higher reactivity of the oxirane group towards the amino than hydroxyl groups.
The organic pollutants present in water, such as bisphenol A, can be removed relatively easily and at a low cost by adsorption processes that can exploit the presence of BCD cage structure immobilized on polymeric supports [35]. In this study, we have determined the quantity of bisphenol A adsorbed per gram of material using ST-HEMA-GMA-BCD materials (Qe (mg bisphenol A/g polymer)). Thus, using a calibration curve for fluorescence intensity depending on the bisphenol A concentration (Supporting info Figure S8), the amount adsorbed onto the BCD modified polymer spheres was determined using Equation (1):
Q e = ( c 0 c e ) × V m
where V is the solution volume (mL), c0 (mg L−1) and ce (mg L−1) are the initial and final solution concentrations of bisphenol A and m is the mass of BCD modified polymer particles (mg).
After 240 min of interaction at 25 °C, the adsorption capacity Qe values obtained were 9.51 and 12.57 mg/g for ST-HEMA-GMA-BCD-OH and ST-HEMA-GMA-BCD-NH2, respectively. The higher Qe value obtained for the polymers modified using the BCD-NH2 can be related to the higher BCD grafting degree. It is easily observed that the large difference in grafting efficiency is in contrast with the relatively small difference between the adsorption capacity at equilibrium. This can be explained by the formation of hydrogen bonds between the hydroxyl groups of BCD-OH and bisphenol A [20]. Nevertheless, the higher bisphenol A adsorption characteristics of ST-HEMA-GMA-BCD-NH2 are evident. Consequently, a kinetic analysis of the adsorption process was performed for ST-HEMA-GMA-BCD-NH2 (Figure 3).
Figure 3 illustrates the adsorption of bisphenol A onto the ST-HEMA-GMA-BCD-NH2 as a function of time in contact. It can be noted that the absorption rate is fast up to 60 min which is followed by a slight decrease up to 200 min, followed by an equilibrium tendency of the system in the 200–300 min. The first stage can be explained by a high bisphenol A concentration in solution which diffuses to the polymer particles surface. The second stage, from 60 to 200 min, represents intermediary behavior during which the adsorption rate decreases as the internal diffusion resistance increases, which is finally followed by the equilibrium characteristics after 200 min. Several mathematical models were analyzed to determine the adsorption efficiency and the mechanism that it follows: Lagergren’s pseudo-first-order kinetic model (Equation (2)), Ho’s pseudo-second-order model (Equation (3)), and Weber’s intra diffusion model (Equation (4)):
ln ( Q e Q t ) = lnQ e k 1 t
t Q t = 1 k 2 Q e 2 + t Q e
Q t = K p t
where Qe (mg g−1) and Qt (mg g−1) are the amounts of bisphenol A adsorbed per unit mass of ST-HEMA-GMA-BCD-NH2 at equilibrium and t (min), respectively. k1 is the pseudo-first-order adsorption rate constant (min−1), k2 is the pseudo-second-order adsorption rate constant (g (mg min)−1), and Kp is the intraparticle diffusion constant (mg g−1 min−0.5).
The kinetic parameters of Lagergren’s pseudo-first-order, Ho’s pseudo-second-order, and Weber’s intra particles diffusion models equations were calculated by slope-intercept of the linear fitting plots of ln(Qe-Qt) versus t, t/Qt versus t, and Qt versus t, respectively (Figure 4).
Comparing the experimental data with the results from the mathematical models for the adsorption process, the best fit was Lagergren’s (both for Qe value and for R2) together with Weber’s intraparticles diffusion model for the step that controls the mass transfer (Figure 3 and Table 1). Analyzing the values for Kp of Weber’s model, this corresponds to a rapid adsorption process in the first stage of contacting [36].
The study of the adsorption isotherms offers information on the interaction between the adsorbate and the adsorbent and allows the determination of the adsorption capacity of the adsorbent, which is an important parameter for system evaluation. The most intensively used isotherm adsorption model are Langmuir (Equation (5)) and Freundlich (Equation (6)).
1 Q e = 1 Q max + 1 Q m K L × 1 c e
lnQ e = lnK F + 1 n lnc e
where Qe (mg g−1) indicates the amount of adsorbate at equilibrium; Qmax (mg g−1) indicates the maximum amount of adsorbate at equilibrium; ce (mg L−1) is the equilibrium concentration of the adsorbate in the solution; KL (L mg−1) and KF (L mg−1) are the Langmuir and Freundlich constants, respectively; and n is the heterogeneity factor.
The isothermal adsorption at the equilibrium of bisphenol A by ST-HEMA-GMA-BCD-NH2 and ST-HEMA-GMA-BCD-OH are represented in (Supporting info Figure S9). From this, it can be noted that the adsorption capacity increases with the increase of adsorbate and reaches saturation as the bisphenol A concentration exceeds 45 mg/L and 40 mg/L in the case of ST-HEMA-GMA-BCD-NH2 and ST-HEMA-GMA-BCD-OH, respectively. The linearization of the two selected isotherms Equation (5), Equation (6), and the parameters calculated are presented in Figure 5 and Table 2.
The comparison of the Langmuir and Freundlich isotherm parameters as listed in Table 2 indicates better linearity in the case of the Langmuir plots, suggesting that the adsorption of bisphenol A by ST-HEMA-GMA-BCD-NH2 and ST-HEMA-GMA-BCD-OH can be regarded as a monolayer adsorption process. This means that the adsorption sites located on the surface of the polymer particles were homogeneously distributed and an equivalent adsorption force is displayed. Additionally, it could be evaluated from the Langmuir equation that the Qmax for bisphenol A was 148.37 mg g−1 and 37.09 mg g−1 for ST-HEMA-GMA-BCD-NH2 and ST-HEMA-GMA-BCD-OH, respectively. (Table 3) For a cross-linked polymer, three main adsorption mechanisms were proposed which involve (1) host–guest interactions in the polymers cavities, (2) interactions in the pores of the polymeric network, and (3) interactions on the surface (physical sorption) [37]. The difference between the adsorption characteristics of the two polymers (Qmax) can be correlated to the amount of BCD grafted to the polymer particles [38]. Thus, due to its higher reactivity, BCD-NH2 afforded a larger substitution degree which is reflected by the enhanced Qmax value.
Comparing the values for Qmax for the adsorption of bisphenol A using different adsorbents (Table 3), it can be noted that the values obtained for our materials are reasonably high. The increased efficiency is due to the high ratio between the specific surface to the mass of the polymer particles and the high reactivity of the surface functional groups (oxirane). These characteristics permit the synthesis of BCD functionalized polymer particles with a good weight ratio (BCD to polymer support) and a proper distribution of BCD on the surface of the polymer particles. Therefore, the possibility of guest–host interaction is facilitated from the steric point of view (see Supplementary Info Figure S10). In addition to this interaction, there is also the possibility for adsorption processes in the pores of the cross-linked polymer particles, respectively physical interaction on the surface of the materials [20]. To confirm the interaction between the polymeric structures modified with BCD and bisphenol A (BPA) FTIR analysis was performed on the materials after the adsorption evaluation. From the spectra (see Supplementary Materials Figure S11), the appearance of a novel signal at 1150 cm−1 corresponding to the C-O vibration from BPA [45] can be observed, confirming the presence of BPA on the surface of the polymer particles.
The thermal resistance is one of the most important properties of polymers and their derivatives, in our case the polymer particles modified with BCD-OH and BCD-NH2. Figure 6 presents the TGA and DTG curves for the synthesized polymers and starting materials.
Comparing the temperatures corresponding for a 10% weight loss (Table 4) it can be noted that BCD-OH has the highest thermal resistance, followed by ST-HEMA-GMA-BCD-OH and ST-HEMA-BCD-NH2, possibly due to the hydrogen bonds formed between the -OH groups. The ST-HEMA and ST-HEMA-GMA display lower thermal stability. The TGA analysis also establishes the temperature where the maximum weight loss takes place. In this case, the Tmax indicated that the most stable materials were ST-HEMA-GMA-BCD-OH and ST-HEMA-GMA-BCD-NH2, which display stability up to 400 °C.

4. Conclusions

A monoamine derivative of BCD was synthesized, characterized by NMR and mass spectroscopy. The BCD derivative was chemically grafted to ST-HEMA-GMA particles obtained by seeded emulsion polymerization. The GMA was used during the seeded polymerization due to its high reactivity towards -OH and NH2 functional groups. The chemical attachment of the BCD derivatives (BCD-OH and BCD-NH2) to the surface of the polymer particles was qualitatively confirmed by FT-IR spectroscopy and quantitatively by acidolysis and phenol colorimetric analysis. The degree of polymer functionalization using the BCD-OH and BCD-NH2 derivatives were 4.27 and 19.19 weight %.
The adsorption properties of the materials were evaluated using bisphenol A as target molecule. The results from the mathematical models for the adsorption kinetics process indicated that the best fit was Lagergren’s model (both for Qe value and for R2), together with Weber’s intraparticles diffusion model for the step that controls the mass transfer in the case of ST-HEMA-GMA-BCD-NH2. The isothermal adsorption evaluation indicated that both systems follow a Langmuir type behavior and afforded a Qmax value of 148.37 mg g−1 and 37.09 mg g−1 for ST-HEMA-GMA-BCD-NH2 and ST-HEMA-GMA-BCD-OH, respectively. Due to the higher reactivity of BCD-NH2, a larger substitution degree of the polymer particles was obtained, which is reflected by the enhanced Qmax value.
The thermogravimetric analysis of the materials indicated that the functionalization of the polymer particles afforded an increase of the thermal resistance. Thus, the BCD modified polymers present a degradation temperature of over 400 °C, which can be attributed to the hydrogen bonds and BCD thermal degradation pathway in the presence of the polymers.

Supplementary Materials

NMR and Maldi characterization Figures S1–S6; UV-Vis and fluorescence determinations procedures and calibration curves (Figure S7 and S8); adsorption isotherms (Figure S9), 3D rendering of bisphenol A insertion in BCD-NH2 (Figure S10) and FTIR spectra of the polymers modified with BCD after BPA adsorption study (Figure S11) are available online at https://www.mdpi.com/article/10.3390/polym13142338/s1.

Author Contributions

Conceptualization, E.R.; methodology, F.R.; software S.B.; validation, E.R., I.M. and A.D.; formal analysis, A.G.; investigation, R.S.; resources, A.M.; data curation, A.D.; writing—original draft preparation, E.R.; writing—review and editing, E.R.; visualization, A.D.; supervision, E.R.; project administration, I.M.; funding acquisition, A.M., A.C.B. All authors have read and agreed to the published version of the manuscript.

Funding

This research received no external funding.

Acknowledgments

Authors are thankful to the POSCCE-O 2.2.1, SMIS-CSNR 13984-901, No. 257/28.09.2010 Project, CERNESIM, for the NMR experiments. Raluca Șomoghi acknowledges financial support by Ministry of Research and Inovation, Nucleu Programme, Project PN.19.23.01.01 Smart-Bi. This work was supported by a grant of the Ministry of Research, Innovation and Digitization, CNCS/CCCDI—UEFISCDI, project number PN-III-P1-1.1-TE-2019-1387 (contract number TE141/2020), within PNCDI III.

Conflicts of Interest

The authors declare no conflict of interest.

References

  1. Ohore, O.E.; Zhang, S. Endocrine disrupting effects of bisphenol A exposure and recent advances on its removal by water treatment systems. A review. Sci. Afr. 2019, 5, e00135. [Google Scholar] [CrossRef]
  2. Bolong, N.; Ismail, A.F.; Salim, M.R.; Rana, D.; Matsuura, T.; Tabe-Mohammadi, A. Negatively charged polyethersulfone hollow fiber nanofiltration membrane for the removal of bisphenol A from wastewater. Sep. Purif. Technol. 2010, 73, 92–99. [Google Scholar] [CrossRef]
  3. Liu, J.; Zhang, L.; Lu, G.; Jiang, R.; Yan, Z.; Li, Y. Occurrence, toxicity and ecological risk of Bisphenol A analogues in aquatic environment—A review. Ecotoxicol. Environ. Saf. 2021, 208, 111481. [Google Scholar] [CrossRef]
  4. Wyżga, B.; Połeć, K.; Olechowska, K.; Hąc-Wydro, K. The impact of toxic bisphenols on model human erythrocyte membranes. Colloids Surf. B Biointerfaces 2020, 186, 110670. [Google Scholar] [CrossRef] [PubMed]
  5. Zhang, H.; Ding, T.; Luo, X.; Li, J. Toxic effect of fluorene-9-bisphenol to green algae Chlorella vulgaris and its metabolic fate. Ecotoxicol. Environ. Saf. 2021, 216, 112158. [Google Scholar] [CrossRef] [PubMed]
  6. Huang, R.-p.; Liu, Z.-h.; Yuan, S.-f.; Yin, H.; Dang, Z.; Wu, P.-x. Worldwide human daily intakes of bisphenol A (BPA) estimated from global urinary concentration data (2000–2016) and its risk analysis. Environ. Pollut. 2017, 230, 143–152. [Google Scholar] [CrossRef] [PubMed]
  7. Sharma, P.; Chadha, P. Bisphenol A induced toxicity in blood cells of freshwater fish Channa punctatus after acute exposure. Saudi J. Biol. Sci. 2021. [Google Scholar] [CrossRef]
  8. Zdarta, J.; Staszak, M.; Jankowska, K.; Kaźmierczak, K.; Degórska, O.; Nguyen, L.N.; Kijeńska-Gawrońska, E.; Pinelo, M.; Jesionowski, T. The response surface methodology for optimization of tyrosinase immobilization onto electrospun polycaprolactone–chitosan fibers for use in bisphenol A removal. Int. J. Biol. Macromol. 2020, 165, 2049–2059. [Google Scholar] [CrossRef]
  9. Fang, Z.; Hu, Y.; Cheng, J.; Chen, Y. Continuous removal of trace bisphenol A from water by high efficacy TiO2 nanotube pillared graphene-based macrostructures in a photocatalytically fluidized bed. Chem. Eng. J. 2019, 372, 581–589. [Google Scholar] [CrossRef]
  10. Yang, S.; Wu, P.; Liu, J.; Chen, M.; Ahmed, Z.; Zhu, N. Efficient removal of bisphenol A by superoxide radical and singlet oxygen generated from peroxymonosulfate activated with Fe0-montmorillonite. Chem. Eng. J. 2018, 350, 484–495. [Google Scholar] [CrossRef]
  11. Zhen, J.; Zhang, S.; Zhuang, X.; Ahmad, S.; Lee, T.; Si, H.; Cao, C.; Ni, S.-Q. Sulfate radicals based heterogeneous peroxymonosulfate system catalyzed by CuO-Fe3O4-Biochar nanocomposite for bisphenol A degradation. J. Water Process Eng. 2021, 41, 102078. [Google Scholar] [CrossRef]
  12. Zahari, A.M.; Shuo, C.W.; Sathishkumar, P.; Yusoff, A.R.M.; Gu, F.L.; Buang, N.A.; Lau, W.-J.; Gohari, R.J.; Yusop, Z. A reusable electrospun PVDF-PVP-MnO2 nanocomposite membrane for bisphenol A removal from drinking water. J. Environ. Chem. Eng. 2018, 6, 5801–5811. [Google Scholar] [CrossRef]
  13. Nasseri, S.; Ebrahimi, S.; Abtahi, M.; Saeedi, R. Synthesis and characterization of polysulfone/graphene oxide nano-composite membranes for removal of bisphenol A from water. J. Environ. Manag. 2018, 205, 174–182. [Google Scholar] [CrossRef] [PubMed]
  14. Liu, Z.; Ye, L.; Xi, J.; Wang, J.; Feng, Z.-g. Cyclodextrin polymers: Structure, synthesis, and use as drug carriers. Prog. Polym. Sci. 2021, 118, 101408. [Google Scholar] [CrossRef]
  15. Luo, Q.; He, L.; Wang, X.; Huang, H.; Wang, X.; Sang, S.; Huang, X. Cyclodextrin derivatives used for the separation of boron and the removal of organic pollutants. Sci. Total Environ. 2020, 749, 141487. [Google Scholar] [CrossRef] [PubMed]
  16. Gaálová, J.; Michel, M.; Bourassi, M.; Ladewig, B.P.; Kasal, P.; Jindřich, J.; Izák, P. Nafion membranes modified by cationic cyclodextrin derivatives for enantioselective separation. Sep. Purif. Technol. 2021, 266, 118538. [Google Scholar] [CrossRef]
  17. Omtvedt, L.A.; Dalheim, M.Ø.; Nielsen, T.T.; Larsen, K.L.; Strand, B.L.; Aachmann, F.L. Efficient Grafting of Cyclodextrin to Alginate and Performance of the Hydrogel for Release of Model Drug. Sci. Rep. 2019, 9, 9325. [Google Scholar] [CrossRef]
  18. Jicsinszky, L.; Martina, K.; Cravotto, G. Cyclodextrins in the antiviral therapy. J. Drug Deliv. Sci. Technol. 2021, 64, 102589. [Google Scholar] [CrossRef] [PubMed]
  19. Morillo, E.; Madrid, F.; Lara-Moreno, A.; Villaverde, J. Soil bioremediation by cyclodextrins. A review. Int. J. Pharm. 2020, 591, 119943. [Google Scholar] [CrossRef]
  20. Gong, T.; Zhou, Y.; Sun, L.; Liang, W.; Yang, J.; Shuang, S.; Dong, C. Effective adsorption of phenolic pollutants from water using β-cyclodextrin polymer functionalized Fe3O4 magnetic nanoparticles. RSC Adv. 2016, 6, 80955–80963. [Google Scholar] [CrossRef]
  21. Mpatani, F.M.; Aryee, A.A.; Kani, A.N.; Guo, Q.; Dovi, E.; Qu, L.; Li, Z.; Han, R. Uptake of micropollutant-bisphenol A, methylene blue and neutral red onto a novel bagasse-β-cyclodextrin polymer by adsorption process. Chemosphere 2020, 259, 127439. [Google Scholar] [CrossRef]
  22. Zhou, Y.; Cheng, G.; Chen, K.; Lu, J.; Lei, J.; Pu, S. Adsorptive removal of bisphenol A, chloroxylenol, and carbamazepine from water using a novel β-cyclodextrin polymer. Ecotoxicol. Environ. Saf. 2019, 170, 278–285. [Google Scholar] [CrossRef]
  23. Xiao, G.; Fu, L.; Li, A. Enhanced adsorption of bisphenol A from water by acetylaniline modified hyper-cross-linked polymeric adsorbent: Effect of the cross-linked bridge. Chem. Eng. J. 2012, 191, 171–176. [Google Scholar] [CrossRef]
  24. Li, X.; Zhou, M.; Jia, J.; Ma, J.; Jia, Q. Design of a hyper-crosslinked β-cyclodextrin porous polymer for highly efficient removal toward bisphenol a from water. Sep. Purif. Technol. 2018, 195, 130–137. [Google Scholar] [CrossRef]
  25. Raza, S.; Wen, H.; Peng, Y.; Zhang, J.; Li, X.; Liu, C. Fabrication of SiO2 modified biobased hydrolyzed hollow polymer particles and their applications as a removal of methyl orange dye and bisphenol-A. Eur. Polym. J. 2021, 144, 110199. [Google Scholar] [CrossRef]
  26. Wang, Z.; Guo, S.; Zhang, B.; Fang, J.; Zhu, L. Interfacially crosslinked β-cyclodextrin polymer composite porous membranes for fast removal of organic micropollutants from water by flow-through adsorption. J. Hazard. Mater. 2020, 384, 121187. [Google Scholar] [CrossRef] [PubMed]
  27. Huang, W.; Hu, Y.; Li, Y.; Zhou, Y.; Niu, D.; Lei, Z.; Zhang, Z. Citric acid-crosslinked β-cyclodextrin for simultaneous removal of bisphenol A, methylene blue and copper: The roles of cavity and surface functional groups. J. Taiwan Inst. Chem. Eng. 2018, 82, 189–197. [Google Scholar] [CrossRef]
  28. Fenyvesi, É.; Barkács, K.; Gruiz, K.; Varga, E.; Kenyeres, I.; Záray, G.; Szente, L. Removal of hazardous micropollutants from treated wastewater using cyclodextrin bead polymer—A pilot demonstration case. J. Hazard. Mater. 2020, 383, 121181. [Google Scholar] [CrossRef]
  29. Tizro, N.; Moniri, E.; Saeb, K.; Panahi, H.A.; Ardakani, S.S. Preparation and application of grafted β-cyclodextrin/thermo-sensitive polymer onto modified Fe3O4@SiO2 nano-particles for fenitrothion elimination from aqueous solution. Microchem. J. 2019, 145, 59–67. [Google Scholar] [CrossRef]
  30. Brady, B.; Lynam, N.; O’Sullivan, T.; Ahern, C.; Darcy, R. β-Cyclodextrin-6 A-(4-methylbenzenesulfonate). Org. Synth. 2000, 77, 220–224. [Google Scholar] [CrossRef]
  31. DuBois, M.; Gilles, K.A.; Hamilton, J.K.; Rebers, P.A.; Smith, F. Colorimetric Method for Determination of Sugars and Related Substances. Anal. Chem. 1956, 28, 350–356. [Google Scholar] [CrossRef]
  32. Rusen, E.; Mocanu, A.; Marculescu, B.; Somoghi, R.; Butac, L.; Miculescu, F.; Cotrut, C.; Antoniac, I.; Cincu, C. Obtaining complex structures starting from monodisperse poly(styrene-co-2-hydroxyethylmethacrylate) spheres. Colloids Surf. A Physicochem. Eng. Asp. 2011, 375, 35–41. [Google Scholar] [CrossRef]
  33. Rusen, E.; Mocanu, A.; Marculescu, B. Obtaining of monodisperse particles through soap-free and seeded polymerization, respectively, through polymerization in the presence of C60. Colloid Polym. Sci. 2010, 288, 769–776. [Google Scholar] [CrossRef]
  34. Ryzhakov, A.; Do Thi, T.; Stappaerts, J.; Bertoletti, L.; Kimpe, K.; Sá Couto, A.R.; Saokham, P.; Van den Mooter, G.; Augustijns, P.; Somsen, G.W.; et al. Self-Assembly of Cyclodextrins and Their Complexes in Aqueous Solutions. J. Pharm. Sci. 2016, 105, 2556–2569. [Google Scholar] [CrossRef]
  35. Simões, S.M.N.; Rey-Rico, A.; Concheiro, A.; Alvarez-Lorenzo, C. Supramolecular cyclodextrin-based drug nanocarriers. Chem. Commun. 2015, 51, 6275–6289. [Google Scholar] [CrossRef]
  36. Wu, F.-C.; Tseng, R.-L.; Juang, R.-S. Initial behavior of intraparticle diffusion model used in the description of adsorption kinetics. Chem. Eng. J. 2009, 153, 1–8. [Google Scholar] [CrossRef]
  37. Ye, H.; Zhao, B.; Zhou, Y.; Du, J.; Huang, M. Recent advances in adsorbents for the removal of phthalate esters from water: Material, modification, and application. Chem. Eng. J. 2021, 409, 128127. [Google Scholar] [CrossRef]
  38. Zhou, Z.; Xiao, Y.; Hatton, T.A.; Chung, T.-S. Effects of spacer arm length and benzoation on enantioseparation performance of β-cyclodextrin functionalized cellulose membranes. J. Membr. Sci. 2009, 339, 21–27. [Google Scholar] [CrossRef]
  39. Gupta, V.K.; Agarwal, S.; Sadegh, H.; Ali, G.A.M.; Bharti, A.K.; Hamdy Makhlouf, A.S. Facile route synthesis of novel graphene oxide-β-cyclodextrin nanocomposite and its application as adsorbent for removal of toxic bisphenol A from the aqueous phase. J. Mol. Liq. 2017, 237, 466–472. [Google Scholar] [CrossRef]
  40. Lin, Q.; Wu, Y.; Jiang, X.; Lin, F.; Liu, X.; Lu, B. Removal of bisphenol A from aqueous solution via host-guest interactions based on beta-cyclodextrin grafted cellulose bead. Int. J. Biol. Macromol. 2019, 140, 1–9. [Google Scholar] [CrossRef]
  41. Kitaoka, M.; Hayashi, K. Adsorption of Bisphenol A by Cross-Linked β-Cyclodextrin Polymer. J. Incl. Phenom. Macrocycl. Chem. 2002, 44, 429–431. [Google Scholar] [CrossRef]
  42. Lee, J.H.; Kwak, S.-Y. Rapid adsorption of bisphenol A from wastewater by β-cyclodextrin-functionalized mesoporous magnetic clusters. Appl. Surf. Sci. 2019, 467–468, 178–184. [Google Scholar] [CrossRef]
  43. Wang, N.; Zhou, L.; Guo, J.; Ye, Q.; Lin, J.-M.; Yuan, J. Adsorption of environmental pollutants using magnetic hybrid nanoparticles modified with β-cyclodextrin. Appl. Surf. Sci. 2014, 305, 267–273. [Google Scholar] [CrossRef]
  44. Shi, S.; Ocampo-Pérez, R.; Lv, J.; Liu, Q.; Nan, F.; Liu, X.; Xie, S.; Feng, J. Diatomite cross-linked β-Cyclodextrin polymers: A novel vision of diatomite adsorbent for the removal of bisphenol A. Environ. Technol. Innov. 2021, 23, 101602. [Google Scholar] [CrossRef]
  45. Ullah, R.; Ahmad, I.; Zheng, Y. Fourier Transform Infrared Spectroscopy of “Bisphenol A”. J. Spectrosc. 2016, 2016, 2073613. [Google Scholar] [CrossRef]
Scheme 1. Synthesis route for BCD-NH2.
Scheme 1. Synthesis route for BCD-NH2.
Polymers 13 02338 sch001
Scheme 2. Chemical synthesis of ST-HEMA-GMA-BCD-NH2. (a) The reaction of BCD-NH2 with ST-HEMA-GMA; (b) ST-HEMA-GMA-BCD-NH2 complex structure (3D).
Scheme 2. Chemical synthesis of ST-HEMA-GMA-BCD-NH2. (a) The reaction of BCD-NH2 with ST-HEMA-GMA; (b) ST-HEMA-GMA-BCD-NH2 complex structure (3D).
Polymers 13 02338 sch002
Figure 1. TEM images of the samples: (a) ST-HEMA; (b) ST-HEMA-GMA; (c) ST-HEMA-GMA-BCD-NH2 and (d) ST-HEMA-GMA-BCD-OH.
Figure 1. TEM images of the samples: (a) ST-HEMA; (b) ST-HEMA-GMA; (c) ST-HEMA-GMA-BCD-NH2 and (d) ST-HEMA-GMA-BCD-OH.
Polymers 13 02338 g001
Figure 2. FT-IR spectra for ST-HEMA, BCD-NH2, ST-HEMA-GMA-BCD-NH2, ST-HEMA-GMA-BCD-OH, ST-HEMA-GMA, ST-HEMA. (a)ST-HEMA; ST-HEMA-GMA; (b) BCD-NH2; ST-HEMA-GMA; Pol-BCD-NH2; Pol-BCD-OH.
Figure 2. FT-IR spectra for ST-HEMA, BCD-NH2, ST-HEMA-GMA-BCD-NH2, ST-HEMA-GMA-BCD-OH, ST-HEMA-GMA, ST-HEMA. (a)ST-HEMA; ST-HEMA-GMA; (b) BCD-NH2; ST-HEMA-GMA; Pol-BCD-NH2; Pol-BCD-OH.
Polymers 13 02338 g002
Figure 3. Adsorption kinetic curve of ST-HEMA-GMA-BCD-NH2 at pH 5 and 25 °C.
Figure 3. Adsorption kinetic curve of ST-HEMA-GMA-BCD-NH2 at pH 5 and 25 °C.
Polymers 13 02338 g003
Figure 4. The linear plots of Lagergren’s pseudo-first-order (A), Ho’s pseudo-second-order (B), and Weber’s intraparticles diffusion models (C).
Figure 4. The linear plots of Lagergren’s pseudo-first-order (A), Ho’s pseudo-second-order (B), and Weber’s intraparticles diffusion models (C).
Polymers 13 02338 g004
Figure 5. (A,C) Langmuir plots illustrating the linear dependences of 1/Qe on 1/ce, and (B,D) Freundlich plot illustrating the linear dependences of lnQe on lnce for adsorption of bisphenol A by ST-HEMA-BCD-NH2 and ST-HEMA-BCD-OH, respectively.
Figure 5. (A,C) Langmuir plots illustrating the linear dependences of 1/Qe on 1/ce, and (B,D) Freundlich plot illustrating the linear dependences of lnQe on lnce for adsorption of bisphenol A by ST-HEMA-BCD-NH2 and ST-HEMA-BCD-OH, respectively.
Polymers 13 02338 g005
Figure 6. (a) TGA curves for BCD-NH2, BCD-OH, ST-HEMA-GMA-BCD-NH2, ST-HEMA-GMA-BCD-OH, ST-HEMA-GMA, ST-HEMA and (b) DTG curves for BCD-NH2, BCD-OH, ST-HEMA-GMA-BCD-NH2, ST-HEMA-GMA-BCD-OH, ST-HEMA-GMA, ST-HEMA.
Figure 6. (a) TGA curves for BCD-NH2, BCD-OH, ST-HEMA-GMA-BCD-NH2, ST-HEMA-GMA-BCD-OH, ST-HEMA-GMA, ST-HEMA and (b) DTG curves for BCD-NH2, BCD-OH, ST-HEMA-GMA-BCD-NH2, ST-HEMA-GMA-BCD-OH, ST-HEMA-GMA, ST-HEMA.
Polymers 13 02338 g006
Table 1. Kinetic parameters for the adsorption of bisphenol A by ST-HEMA-GMA-BCD-NH2.
Table 1. Kinetic parameters for the adsorption of bisphenol A by ST-HEMA-GMA-BCD-NH2.
Lagergren’s Pseudo-First-OrderHo’s Pseudo-Second-Order ModelWeber’s Intraparticles Diffusion Model
Qe, exp (mg g−1)k1 × 103
(min−1)
Qe
(mg g−1)
R2k2 × 103
(g mg−1 min−1)
Qe
(mg g−1)
R2Kp
(mg g−1 min−0.5)
R2
12.574.712.360.9332.18.790.90540.508730.9882
Table 2. Isotherm parameters for the adsorption of bisphenol A by ST-HEMA-GMA-BCD-NH2 and ST-HEMA-GMA-BCD-OH.
Table 2. Isotherm parameters for the adsorption of bisphenol A by ST-HEMA-GMA-BCD-NH2 and ST-HEMA-GMA-BCD-OH.
AbsorbentAdsorbateLangmuirFreundlich
KL/
(L mg)−1
Qmax/
(mg g−1)
R2KF/
(L mg−1)
nR2
ST-HEMA-GMA-BCD-NH2Bisphenol A0.0025148.370.94310.61832.2680.9244
ST-HEMA-GMA-BCD-OHBisphenol A0.019537.090.95051.91791.74780.9376
Table 3. Comparison of adsorption capacities of different polymer adsorbents for bisphenol A.
Table 3. Comparison of adsorption capacities of different polymer adsorbents for bisphenol A.
AdsorbentPhenolic PollutantsQmax (mg g−1)Reference
Hyper-crosslinked β-CD porous polymerBisphenol A278[24]
Graphene oxide-β-CD nanocompositesBisphenol A373.4[39]
BCD polymer functionalized Fe3O4 magnetic nanoparticlesBisphenol A74.63[20]
BCD grafted cellulose beadsBisphenol A30.77[40]
(BCD+epichlorohydrin) polyBCDBisphenol A84[41]
BCD-Functionalized
Mesoporous Magnetic Clusters
Bisphenol A52.7[42]
BCD-poly(glycidyl methacrylate)-SiO2- nanoparticlesBisphenol A22.48[43]
Diatomite cross-linked BCD polymersBisphenol A83.57[44]
ST-HEMA-GMA-BCD-NH2Bisphenol A148.37This study
ST-HEMA-GMA-BCD-OHBisphenol A37.09This study
Table 4. Thermal properties of BCD-NH2, BCD-OH, ST-HEMA-GMA-BCD-NH2, ST-HEMA-GMA-BCD-OH, ST-HEMA-GMA, ST-HEMA.
Table 4. Thermal properties of BCD-NH2, BCD-OH, ST-HEMA-GMA-BCD-NH2, ST-HEMA-GMA-BCD-OH, ST-HEMA-GMA, ST-HEMA.
SampleT10%, [°C]Tmax, [°C]
ST-HEMA283283; 355; 373
ST-HEMA-GMA244257; 409
BCD-NH2172310
BCD-OH306318
ST-HEMA-GMA-BCD-OH303313; 425
ST-HEMA-GMA-BCD-NH2291299; 424
T10% = decomposition onset temperature (measured at 10% weight loss); Tmax = the maximum decomposition temperature, corresponding to the maximum of DTG peak (the first derivative of the thermogravimetric curve).
Publisher’s Note: MDPI stays neutral with regard to jurisdictional claims in published maps and institutional affiliations.

Share and Cite

MDPI and ACS Style

Bucur, S.; Mangalagiu, I.; Diacon, A.; Mocanu, A.; Rizea, F.; Somoghi, R.; Ghebaur, A.; Boscornea, A.C.; Rusen, E. Novel Chemical Architectures Based on Beta-Cyclodextrin Derivatives Covalently Attached on Polymer Spheres. Polymers 2021, 13, 2338. https://doi.org/10.3390/polym13142338

AMA Style

Bucur S, Mangalagiu I, Diacon A, Mocanu A, Rizea F, Somoghi R, Ghebaur A, Boscornea AC, Rusen E. Novel Chemical Architectures Based on Beta-Cyclodextrin Derivatives Covalently Attached on Polymer Spheres. Polymers. 2021; 13(14):2338. https://doi.org/10.3390/polym13142338

Chicago/Turabian Style

Bucur, Stefan, Ionel Mangalagiu, Aurel Diacon, Alexandra Mocanu, Florica Rizea, Raluca Somoghi, Adi Ghebaur, Aurelian Cristian Boscornea, and Edina Rusen. 2021. "Novel Chemical Architectures Based on Beta-Cyclodextrin Derivatives Covalently Attached on Polymer Spheres" Polymers 13, no. 14: 2338. https://doi.org/10.3390/polym13142338

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.

Article Metrics

Back to TopTop