Next Article in Journal
Microstructural Stability and Softening Resistance of a Novel Hot-Work Die Steel
Next Article in Special Issue
Abrupt Change Effect of Bandgap Energy on Quantum System of Silicon Nanowire
Previous Article in Journal
The Investigation for Coating Method of Titanium Dioxide Layer in Perovskite Solar Cells
Previous Article in Special Issue
Formation of Dislocations in the Growth of Silicon along Different Crystallographic Directions—A Molecular Dynamics Study
 
 
Font Type:
Arial Georgia Verdana
Font Size:
Aa Aa Aa
Line Spacing:
Column Width:
Background:
Article

Synthesis of Boron-Doped Silicon Film Using Hot Wire Chemical Vapor Deposition Technique

1
Department of Physics, BSMR Maritime University, Dhaka 1216, Bangladesh
2
Department of Physics, University of Mumbai, Mumbai 400098, India
*
Author to whom correspondence should be addressed.
Crystals 2020, 10(4), 237; https://doi.org/10.3390/cryst10040237
Submission received: 5 February 2020 / Revised: 15 March 2020 / Accepted: 16 March 2020 / Published: 25 March 2020
(This article belongs to the Special Issue Growth and Evaluation of Crystalline Silicon (Volume II))

Abstract

:
Boron-doped polycrystalline silicon film was synthesized using hot wire chemical vapor deposition technique for possible application in photonics devices. To investigate the effect of substrate, we considered Si/SiO2, glass/ITO/TiO2, Al2O3, and nickel tungsten alloy strip for the growth of polycrystalline silicon films. Scanning electron microscopy, optical reflectance, optical transmittance, X-ray diffraction, and I-V measurements were used to characterize the silicon films. The resistivity of the film was 1.3 × 10−2 Ω-cm for the polycrystalline silicon film, which was suitable for using as a window layer in a solar cell. These films have potential uses in making photodiode and photosensing devices.

1. Introduction

Hydrogenated intrinsic polysilicon film can reduce the cost of optoelectronics device significantly. The prospects of intrinsic polysilicon films for thin-film solar cell and other optoelectronic device fabrication using hot wire chemical vapor deposition (HWCVD) were well evaluated [1]. The intrinsic silicon film requires controlled doping to make the films suitable for optoelectronic device application. Boron-doped highly conducting 0.08 (Ωcm)−1 polycrystalline silicon films were optimized using HWCVD for solar cell application [2,3,4]. Thin-film solar cell fabricated on plastic substrate at 150 °C also showed the prospect of these films as a cost-effective solution [5]. In this article, we described the growth, optimization, and characterization of boron-doped polycrystalline silicon films synthesized using HWCVD. To investigate the effect of nature of substrate on crystallinity of grown boron-doped silicon film, we considered four different substrates, silicon dioxide on silicon wafer (Si/SiO2), titanium dioxide on glass (glass/ITO/TiO2), sapphire (Al2O3), and nickel–5%tungsten alloy textured metal strip (Ni-W) with dominant (002) orientation. Basic motivation for carrying out growth on different types of substrates came from the works of Green et al. [6], Teplin et al. [7], and Findikoglu et al. [8], who showed growth of textured silicon films on amorphous substrates. SiO2 on Si is an amorphous substrate. Sapphire is chosen as a robust substrate and Ni-W is chosen as a flexible substrate. A range of experiments were conducted by varying the growth conditions to optimize the crystalline quality of silicon film with an intention to use the film in a solar cell [9,10]. Thin-film solar cells of p-i-n structure have i-layer as the light absorber and p-type layer as a window. At the initial stage, we conducted experiments for the synthesis of p-type polycrystalline silicon layers on a variety of substrates.

2. Experimental Section

2.1. HWCVD System Used for Synthesis and Other Apparatus

The HWCVD system used in this work [11] was custom made of stainless steel with provision of a window for monitoring the tungsten filament temperature. Single filament of tungsten wire, 65 cm long and 0.5 mm in diameter, wound in a zigzag shape was resistively heated to 1900 °C using a DC power supply. The filament was placed at about 5 cm height above the substrate. The area covered by the filament was about 9 cm × 9 cm. The hot filament radiatively heated the substrate to 200 °C as measured with a thermocouple in contact with the substrate surface in a temperature calibration run. Higher substrate temperature was achieved by a resistive heater placed in contact with the substrate holder from below. A moveable shutter between the wire and the substrate allowed several growth steps to be performed with definite starting and ending point for each step during the growth of the film. The gas flow shower was located above the filament. The vacuum system had base pressure of 1 × 10−6 mbar, and it was equipped with a load lock to avoid exposing the system to room ambient while loading and unloading the samples. A mixture of pure SiH4 and pure H2 was used as a process gas for the intrinsic silicon film. Diborane (5% diborane and 95% hydrogen) gas was introduced as a source of boron for p-type silicon film. For film thickness measurement, a DektakXT stylus profiler, from Bruker, Billerica, MA, USA, was used.
Si/SiO2 substrates were prepared by oxidizing 500 nm of silicon dioxide on 2-inch (100) silicon wafers using a wet oxidation process. We used one-fourth of the 2-inch diameter silicon wafer for the growth process. Sapphire (Al2O3) substrates were 1 cm × 2 cm and were cut from 0.5 mm thick, c-axis oriented, both sides polished, two inch diameter wafer, and were obtained from Semiconductor Wafer Inc. Titanium dioxide (TiO2) substrates (1 cm × 2 cm) were (112) oriented anatase, prepared by atmospheric chemical vapor deposition (ACVD) techniques, on indium tin oxide (ITO)-coated glass, and were synthesized at the Washington University [12]. The interest in this substrate was not for optoelectronics, but for its application as electrode for energy storage. We used nickel–5% tungsten (Ni-W) metal tape (1 cm × 2 cm) [13] of about 80-micron thickness, biaxially textured Ni-W substrates with dominant (002) orientation, obtained from EVICO GmbH, as metal substrate.

2.2. Growth of Boron-Doped Polycrystalline Silicon Film

The growth began with a nucleation step at 400 °C. This was based on the experiments of Vallat-Sauvain et al. [14] who showed that the silicon grains synthesized by Plasma Enhanced Chemical Vapor Deposition (PECVD), using a dilute mixture of silane with hydrogen, developed preferential (220) orientation for a certain ratio of SiH4/H2 precursors. In our experiments, we used H2:SiH4 in the ratio of 20:1 for duration of 100 s.
Boron-doped silicon films were grown on various substrates using HWCVD, starting with a thin silicon nucleation layer at 400 °C substrate temperature. The substrate temperature was ramped from 400 °C to 600 °C for higher surface mobility of silicon atoms to continue the growth. Table 1 shows the growth conditions for the thin and thick film, respectively.
The growth of boron-doped polysilicon layer was done by two schemes. In the first scheme, the gas mixture remained the same as used for the nucleation stage. In the second scheme, the growth of silicon layer proceeded in five stages after the nucleation stage, with gradual increasing concentration of SiH4 as listed in Table 1. The silane flow rate was increased in steps while simultaneously decreasing the H2 flow rate in order to keep the chamber pressure constant. To facilitate the measurement of thickness, we placed a piece of silicon, covering one end of the Si/SiO2 substrate, as mask. This allowed us to measure the step height using surface profiler. The thickness, as shown in the Table 1, is for the boron-doped silicon film on Si/SiO2 substrate.

3. Results and Discussion

3.1. SEM Image Analysis

We took scanning electron microscope (Zeiss Ultra 55 SEM with Oxford EDX) images to observe the grain size and shape in p-type polycrystalline silicon films.
Figure 1 shows morphology of silicon thin films grown on different substrates following the recipe given in Table 1, Experiment Number 1. Films on Si/SiO2 and Al2O3 substrate had similar shaped circular grains with average grain size of 30 nm. Grains on glass/ITO/TiO2 substrate were not circular in shape and average grain size was larger, about 100 nm. The shape of crystalline grains on nickel substrate was rather different from the shapes observed in all other substrates. Grains were randomly oriented, merged together to form larger grains of 400 nm, and in some portion, a columnar growth was also observed.
Figure 2 shows morphology of thick polycrystalline silicon film grown on different substrates following the recipe given in Table 1, Experiment Number 2. Films grown on Si/SiO2, glass/ITO/TiO2 and Al2O3 substrates had grain size of 100 nm, and the shapes were similar to those observed in the case of intrinsic silicon film [15]. Grains on nickel substrate looked different. Grains were merged and two to three microns in size. Sharp, pointed four-micron features were observed due to the contribution from the Ni-W substrate effect. We looked at the TEM of undoped silicon films grown on Si/SiO2 substrate using the same gas mixture, except for diborane, and same growth procedure [16]. The nucleation layer was about 10 nm thick. The layer immediately above the nucleation layer, about 0.2 micron thick, was of very high crystalline quality as seen from selective area diffraction (spotty pattern). The top layer, however, had more polycrystalline nature (rings diffraction pattern). This aspect requires further investigation.

3.2. Crystal Orientation

Structural characterization of silicon films was performed using CuKα radiation from high-resolution X-ray diffraction (XRD) instrument, SmartLab 3 kW, from Rigaku Corporation, Japan, operated at 40 keV, 40 mA, and CuKα in θ–2θ geometry. XRD measurements for thick boron-doped polycrystalline silicon film grown on Si/SiO2, glass/ITO/TiO2, Al2O3, and Ni-W substrates are shown in Figure 3. All the data were taken at 2θ in the range of 20°–60°. XRD patterns contained peaks corresponding to the silicon film as well as the substrates. Broad hump in XRD of the Si/SiO2 substrate at 2θ less than 36° was due to the scattering from amorphous SiO2. Some of the substrate peaks were marked in Figure 3. Strong peaks corresponding to the sapphire and (002) textured Ni-W substrates appeared at 2θ equal to 42° and 51°, respectively, which were removed to facilitate the presentation. For analysis purpose, we considered the three peaks at 2θ values of 28.5°, 47.5°, and 56° for the boron-doped polycrystalline silicon planes (111), (220), and (311), respectively. The peaks corresponding to (220) increased significantly for silicon film on Si/SiO2, glass/ITO/TiO2, and Al2O3 substrates. Hence for thick boron-doped polycrystalline silicon film (220), a preferred growth direction was observed. Boron-doped polycrystalline silicon film on Ni-W substrate showed no preferred crystal orientation. This result was different from the result of Teplin et al. [7], who obtained nearly epitaxial films using several intermediate oxide layers. It was possible that silicon reacted with nickel, and prevented growth of silicon nuclei in the initial stages so that the growth turned out to be random.

3.3. Optical Transmission and Reflectance

Transmission and reflectance spectra allowed us to evaluate the optical properties of boron-doped silicon films in the Ultraviolet-Visible-Near Infrared (UV-VIS-NIR) range of wavelengths. We took transmittance and reflectance spectra for the silicon film on sapphire (Al2O3) substrates using PVE300 spectrometer from Bentham Inst. Ltd., and these are shown in Figure 4. Interference oscillations were observed at wavelengths longer than 500 nm for silicon film on sapphire substrates as the film on this substrate was smooth. No transmission measurement was performed for the silicon films deposited on Si/SiO2 and nickel substrates, since these substrates absorb light of wavelengths in the range of interest. Reflectance spectrum measured on Si/SiO2 substrate was similar to that measured on the sapphire substrate. The overall reflection was 30% or lower.
These experiments showed that optical quality of film is suitable for use in a p-i-n solar cell with the thickness modified as required by the device design.

3.4. Resistivity Analysis

Sheet resistivity and bulk resistivity of the films were measured using collinear four-point probe apparatus by Lucas-Signatone Corp. The measurements for boron-doped silicon film grown on Si/SiO2 and on sapphire substrates are shown in Table 2. In comparison, the resistivity of undoped films was about 2–4 × 105 ohm-cm (these measurements were done with deposited contacts using electrometer) [15]. Doping with boron lowered the resistivity by several orders of magnitude as expected. Relatively higher resistivity was observed for thick polycrystalline silicon film on 2_Si/SiO2 and 30_Al2O3 substrate compared to the thin silicon film. This may be due to the change in the gas composition for thicker growth, with larger silane content and corresponding reduction in the diborane to silane ratio. As given in Section 3.1, the TEM results showed better crystallinity for the layer adjacent to the nucleation layer. This may be also contributed to the differences in the resistivity. From the EDX measurement, the presence of oxygen was noticed though we took it as contamination. No I-V measurements were done on p-type silicon film on nickel and glass/ITO/TiO2 substrates using four-probe setup because these substrates had back conducting metal.

4. Conclusions

Our experiments showed that one-micron thick p-type boron-doped silicon films prepared at 600 °C are preferentially oriented along (220) direction. We achieved fairly high average growth rates (about 7 A°/s) for the thick films by increasing the silane content in the gas mixture. However, the average grain size remained small on Si/SiO2 and Al2O3 substrates. The resistivity of the thin films was in the range of 1.3–1.7 × 10−2 Ω-cm, while in the thicker films, the resistivity was in the range of 4.64–7.88 × 10−2 Ω-cm. This increase in resistivity was may be due to the reduction in the ratio of diborane to silane by a factor of 5 in the thicker films compared to that in the thinner films. By optimizing the thickness and doping concentration, these films can have potential application in optoelectronics devices.

Author Contributions

Both the authors M.A.H., and B.M.A. participated in the conceptualization, designing methodology, analysis, interpretation, discussion and improvement of the manuscript of the experimental data on synthesis of boron doped polycrystalline silicon film. M.A.H. collected and analyzed the data followed by the manuscript preparation while B.M.A. does the review, editing, supervision and funding acquisition. All the figures and images are prepared by M.A.H. Both the authors have read and agreed to the published version of the manuscript.

Funding

This research was funded by Centre of Excellence in Nanoelectronics (CEN) of the Indian Institute of Technology, Bombay, Mumbai, India.

Acknowledgments

The authors would like to thank K.L. Narasimhan for enlightening discussions at every stage of this work. The authors thank HWCVD system team Anjum A., Poonam K., and Raorane of the Centre of Excellence in Nanoelectronics (CEN) of the Indian Institute of Technology, Bombay, and the team doing XRD and electron microscope measurements at the Tata Institute of Fundamental Research, Mumbai.

Conflicts of Interest

The authors declare no conflict of interest. The funders had no role in the design of the study; in the collection, analyses, or interpretation of data; in the writing of the manuscript, or in the decision to publish the results.

References

  1. Waman, V.S.; Funde, A.M.; Kamble, M.M.; Pramod, M.R.; Hawaldar, R.R.; Amalnerkar, D.P.; Sathe, V.G.; Gosavi, S.W.; Jadkar, S.R. Hydrogenated Nano crystalline Silicon Thin Films Prepared by Hot-Wire Method with Varied Process Pressure. J. Nanotechnol. 2011. [Google Scholar] [CrossRef] [Green Version]
  2. Jadkar, S.R.; Sali, J.V.; Takwale, M.G.; Musale, D.V.; Kshirsagar, S.T. Synthesis of highly conductive boron-doped p-type hydrogenated microcrystalline silicon (μc-Si:H) by a hot-wire chemical vapor deposition technique. Sol. Energy Mater. Sol. Cells 2000, 64, 333–346. [Google Scholar] [CrossRef]
  3. Zhang, C.; Meier, M.; Lambertz, A.; Smirnov, V.; Holländer, B.; Gordijn, A.; Merdzhanova, T. Optical and Electrical Effects of p-type μc-SiOx:H in Thin-Film Silicon Solar Cells on Various Front Textures. Int. J. Photoenergy 2014. [Google Scholar] [CrossRef]
  4. Fathi, E.; Vygranenko, Y.; Vieira, M.; Sazonov, A. Boron-doped nanocrystalline silicon thin films for solar cells. Appl. Surf. Sci. 2011, 257, 8901–8905. [Google Scholar] [CrossRef] [Green Version]
  5. Filonovich, S.A.; Alpuim, P.; Rebouta, L.; Bourée, J.-E.; Soro, Y.M. Hydrogenated amorphous and nanocrystalline silicon solar cells deposited by HWCVD and RF-PECVD on plastic substrates at 150 °C. J. Non-Cryst. Solids 2008, 354, 2376–2380. [Google Scholar] [CrossRef]
  6. Green, M.A.; Basore, P.A.; Chang, N.; Clugston, D.; Egan, R.; Evans, R.; Hogg, D.; Jarnason, S.; Keevers, M.; Lasswell, P.; et al. Crystalline silicon on glass (CSG) thin-film solar cell modules. Sol. Energy 2004, 77, 857–863. [Google Scholar] [CrossRef]
  7. Teplin, C.W.; Ginley, D.S.; Branz, H.M. A new approach to thin film crystal silicon on glass: Biaxially-textured silicon on foreign template layers. J. Non-Cryst. Solids 2006, 352, 984–988. [Google Scholar] [CrossRef]
  8. Findikoglu, A.T.; Choi, W.; Matias, V.; Holesinger, T.G.; Jia, Q.X.; Peterson, D.E. Well-Oriented Silicon Thin Films with High Carrier Mobility on Polycrystalline Substrates. Adv. Mater. 2005, 17, 1527–1531. [Google Scholar] [CrossRef]
  9. Park, J.; Shin, C.; Park, H.; Jung, J.; Lee, Y.-J.; Bong, S.; Dao, V.A.; Balaji, N.; Yi, J. Boron Doped Nanocrystalline Film with Improved Work Function as a Buffer Layer in Thin Film Silicon Solar Cells. Nano Sci. Nano Technol. 2015, 15, 2241–2246. [Google Scholar] [CrossRef] [PubMed]
  10. Hsu, C.-H.; Zhang, X.-Y.; Zhao, M.J.; Lin, H.-J.; Zhu, W.-Z.; Lien, S.-Y. Silicon Heterojunction Solar Cells with p-Type Silicon Carbon Window Layer. Crystals 2019, 9, 402. [Google Scholar] [CrossRef] [Green Version]
  11. Kale, N. Making Hotwire CVD a Viable Technology Alternative for Bio-MEMS Applications: Device Optimization, Fabrication and Characterization. Ph.D. Thesis, IIT Bombay, Mumbai, India, 2008. [Google Scholar]
  12. Chadha, T.S.; Dutta, P.K.; Raliya, R.; Mitra, S.; Biswas, P. Sustainable one step process for making carbon-free TiO2 anodes and sodium-ion battery electrochemistry. Sustain. Energy Fuels 2018, 2, 1582–1587. [Google Scholar] [CrossRef]
  13. Wee, S.H.; Cantoni, C.; Fanning, T.R.; Teplin, C.W.; Bogorin, D.F.; Bornstein, J.; Bowers, K.; Schroeter, P.; Hasoon, F.; Branz, H.M.; et al. Hetero epitaxial film silicon solar cell grown on Ni-W foils. Energy Environ. Sci. 2012, 5, 6052–6056. [Google Scholar] [CrossRef]
  14. Vallat-Sauvain, E.; Kroll, U.; Meier, J.; Shah, A.; Pohl, J. Evolution of the microstructure in microcrystalline silicon prepared by very high frequency glow-discharge using hydrogen dilution. J. Appl. Phys. 2000, 87, 3137–3142. [Google Scholar] [CrossRef] [Green Version]
  15. Kaur, G.; Hossion, M.A.; Kulasekaran, M.; Arora, B.M. Synthesis of oriented and passivated polycrystalline silicon films on glass by hot wire chemical vapor deposition. In Proceedings of the 2014 IEEE 40th Photovoltaic Specialist Conference (PVSC), Denver, CO, USA, 8–13 June 2014; pp. 1326–1328. [Google Scholar] [CrossRef]
  16. Hossion, A.; Arora, B.M. Cross Sectional TEM Characterization of Epitaxial Silicon Film Grown using Hot Wire Chemical Vapor Deposition. J. Thin Film Sci. Technol. 2020, 9, 37–40. Available online: http://www.naturalspublishing.com/Article.asp?ArtcID=20407 (accessed on 2 February 2020).
Figure 1. SEM image of boron-doped p-type polycrystalline silicon thin film (Exp. 1) on (a) Si/SiO2, (b) Al2O3, (c) glass/ITO/TiO2, and (d) Ni-W.
Figure 1. SEM image of boron-doped p-type polycrystalline silicon thin film (Exp. 1) on (a) Si/SiO2, (b) Al2O3, (c) glass/ITO/TiO2, and (d) Ni-W.
Crystals 10 00237 g001
Figure 2. SEM image of boron-doped p-type polycrystalline silicon thick film (Exp. 2) on (a) Si/SiO2, (b) Al2O3, (c) glass/ITO/TiO2, and (d) Ni-W substrates.
Figure 2. SEM image of boron-doped p-type polycrystalline silicon thick film (Exp. 2) on (a) Si/SiO2, (b) Al2O3, (c) glass/ITO/TiO2, and (d) Ni-W substrates.
Crystals 10 00237 g002
Figure 3. Diffraction spectrum of thick boron-doped polycrystalline silicon film on (a) 29_Ni-W-pSi, (b) 27_ Glass/ITO/TiO2-pSi, (c) 30_Sapphire-pSi (Al2O3), and (d) 2_Si/SiO2-pSi substrate.
Figure 3. Diffraction spectrum of thick boron-doped polycrystalline silicon film on (a) 29_Ni-W-pSi, (b) 27_ Glass/ITO/TiO2-pSi, (c) 30_Sapphire-pSi (Al2O3), and (d) 2_Si/SiO2-pSi substrate.
Crystals 10 00237 g003
Figure 4. Reflectance spectrum of boron-doped p-type polycrystalline silicon film on sapphire (Al2O3) substrates. Transmission spectrum of boron-doped p-type polycrystalline silicon film on sapphire (Al2O3) substrates.
Figure 4. Reflectance spectrum of boron-doped p-type polycrystalline silicon film on sapphire (Al2O3) substrates. Transmission spectrum of boron-doped p-type polycrystalline silicon film on sapphire (Al2O3) substrates.
Crystals 10 00237 g004
Table 1. Growth parameter of boron-doped p-type polycrystalline silicon films on Si/SiO2, sapphire (Al2O3), glass/ITO/TiO2, and Ni-W substrates.
Table 1. Growth parameter of boron-doped p-type polycrystalline silicon films on Si/SiO2, sapphire (Al2O3), glass/ITO/TiO2, and Ni-W substrates.
Exp. No.Sample NameProcess Pressure in mbarSubstrate Temp. in °CGas Flow in Sccm
H2:SiH4:5%B2H6
Growth Duration in SecFilm Thickness in nm
Two-stage growth (thin film)
118_Si/SiO2
24_Al2O3
25_Glass/ITO/TiO2
26_Ni-W
2.4 × 10−140015:1:5110218
2.5 × 10−160015:1:51000
Six-stage growth (thick film)
22_Si/SiO2
27_Glass/ITO/TiO2
29_Ni-W
30_ Al2O3
2.3 × 10−140015:1:51001085
2.1 × 10−1
to
2.3 × 10−1
60015:1:5100
15:1.5:5100
13:2:5100
12:3:5100
10:5:51000
Table 2. Resistivity of boron-doped silicon film on Si/SiO2 and Al2O3 substrates.
Table 2. Resistivity of boron-doped silicon film on Si/SiO2 and Al2O3 substrates.
Sample NameVoltage
Volt (V)
Current Amp (I)Sheet Resistance = (V × 4.532)/I
ohm/square
Thickness cmResistivity Ohm-cm
Polycrystalline silicon thin film
18_Si/SiO21.351 × 10−26.12 × 1022.18 × 10−51.33 × 10−2
24_Al2O31.671 × 10−27.6 × 1022.18 × 10−51.65 × 10−2
Polycrystalline silicon thick film
2_Si/SiO20.931 × 10−24.2 × 1021.1 × 10−44.64 × 10−2
30_Al2O31.581 × 10−27.2 × 1021.1 × 10−47.88 × 10−2

Share and Cite

MDPI and ACS Style

Hossion, M.A.; Arora, B.M. Synthesis of Boron-Doped Silicon Film Using Hot Wire Chemical Vapor Deposition Technique. Crystals 2020, 10, 237. https://doi.org/10.3390/cryst10040237

AMA Style

Hossion MA, Arora BM. Synthesis of Boron-Doped Silicon Film Using Hot Wire Chemical Vapor Deposition Technique. Crystals. 2020; 10(4):237. https://doi.org/10.3390/cryst10040237

Chicago/Turabian Style

Hossion, M. Abul, and B. M. Arora. 2020. "Synthesis of Boron-Doped Silicon Film Using Hot Wire Chemical Vapor Deposition Technique" Crystals 10, no. 4: 237. https://doi.org/10.3390/cryst10040237

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.

Article Metrics

Back to TopTop