Nysfungin Production Improvement by UV Mutagenesis in Streptomyces noursei D-3-14
 
 
Font Type:
Arial Georgia Verdana
Font Size:
Aa Aa Aa
Line Spacing:
Column Width:
Background:
Article

Methanol Steam Reforming over La1-xSrxCeO3-δ Catalysts for Hydrogen Production: Optimization of Operating Parameters

Marine Engineering College, Dalian Maritime University, Dalian 116026, China
*
Author to whom correspondence should be addressed.
Catalysts 2023, 13(2), 248; https://doi.org/10.3390/catal13020248
Submission received: 26 December 2022 / Revised: 14 January 2023 / Accepted: 19 January 2023 / Published: 21 January 2023

Abstract

:
In this study, a series of A-site strontium-doped La1-xSrxCeO3-δ (x = 0.2, 0.4, 0.6, 0.8) perovskite catalysts were synthesized via the ethylenediaminetetraacetic acid (EDTA) sol-gel method for hydrogen production by methanol steam reforming. The fresh and the reduced catalysts are characterized by scanning X-ray (XRD), energy dispersive X-ray spectroscopy (EDS) and scanning electron microscopy (SEM) techniques. Results showed that La0.6Sr0.4CeO3-δ exhibited the best performance among the La1-xSrxCeO3-δ catalysts. The operating parameters were optimized to study the catalytic performance of La0.6Sr0.4CeO3-δ, including catalytic temperature, water–methanol ratio (W/M) and liquid hourly space velocity (LHSV). However, the excessive strontium content led to a decrease in hydrogen production amount per unit time, and the high W/M promoted the reverse water–gas shift reaction (RWGS), which resulted in a decrease in CO selectivity and an increase in CO2 selectivity. In addition, the optimal reaction parameters are as follows: reforming temperature of 700 °C; W/M of 3:1; LHSV of 20 h−1. Furthermore, the methanol conversion rate of La0.6Sr0.4CeO3-δ can reach approximately 82%, the hydrogen production can reach approximately 3.26 × 10−3 mol/g(cat)/min under the optimum reaction conditions. Furthermore, La0.6Sr0.4CeO3-δ exhibits high hydrogen selectivity (85%), which is a promising catalyst for MSR application.

1. Introduction

Hydrogen is considered an efficient and clean energy that is a promising alternative energy to fossil fuels. Hydrogen combustion can generate higher energy density, along with water, and will not produce greenhouse gases such as carbon dioxide, rendering it a form of clean energy [1]. Meanwhile, hydrogen is considered the key pathway for deep decarbonization in the energy and transportation sectors, which is widely utilized in the chemical and petroleum industries. It was also identified as one of the most promising clean energy sources for power generation and fuel cell equipment [2].
Although hydrogen shows great potential as an alternative energy source, it still faces many challenges, such as storage and transportation of hydrogen being major limitations and the need for high pressure and low temperature conditions for hydrogen storage systems compared to conventional fuels, which will make production more expensive and dangerous [3]. In order to overcome these challenges, researchers have combined renewable energy with hydrogen energy and conducted much research on new fuels that can provide hydrogen-rich gas for fuel cells. At present, liquid fuel as a hydrogen carrier is a promising way to produce on-line hydrogen for vehicles or other devices [4]. Among them, methanol has received extensive attention. At room temperature, methanol is a liquid without C-C bonds that is easy to store and transport. It has high H/C ratio, high hydrogen content, high energy density and high hydrogen yield, and the methanol hydrogen production device is relatively simple. In addition, methanol is also a carbon neutral renewable raw material, and its production is also economically sustainable, as it can be prepared from fossil resources as well as biomass. Methanol dry reforming (DR) [5], methanol steam reforming (MSR) [6], methanol partial oxidation (POX) [7], and methanol self-thermal reforming (ATR) [8] are currently the four main methods utilized to transform methanol into hydrogen-rich gas. When compared to the other technologies, MSR has some advantages due to its low CO yield and high H/C ratio [9]. Furthermore, the MSR process involves a simpler catalytic reaction and easier temperature control. The MSR reaction can be represented by (Equation (1)). However, there are two common side reactions in the MSR reaction, the direct methanol decomposition reaction (Equation (2)) and the water–gas conversion inverse reaction (Equation (3)). Special attention should be paid to the concentration of CO in the reaction, as CO can be hazardous to the electrical electrodes of the fuel cell.
CH3OH + H2O → CO2 + 3H2 ΔH◦ = +50 kJ·mol−1
CH3OH → CO + 2H2 ΔH◦ = +91 kJ·mol−1
CO2 + H2 → CO + H2O ΔH◦ = +41 kJ·mol−1
The reaction performance of MSR mainly depends on the catalyst, thus, an ideal catalyst could avoid side reactions, prevent deactivation caused by carbon deposition, and improve the selectivity of hydrogen. Due to their distinctive crystal structure and catalytic properties, perovskite oxides (ABO3) have attracted a lot of attention. A-site is an alkaline earth or rare earth element, while B-site is typically a transition element. Both A- and B-sites can be partially replaced by metal ions, which will change their catalytic, structural and redox properties, thus, improving catalytic activity and stability.
Wu et al. [10] synthesized La1-xCaxNiO3 perovskite-type oxides. The results indicated that the doping of Ca at A-site resulted in a strong metal–carrier interaction and produced a high metal dispersion, which inhibited the deposition of carbon and improved the stability of the catalyst. Zhang et al. [11] synthesized LaNiO3-δ nanoparticles that were undoped and doped with strontium by the sol-gel method. The results indicated that strontium doping can introduce more oxygen vacancies in LaNiO3-δ, and catalytic performance than undoped LaNiO3-δ. Morales et al. [12] prepared La0.6Sr0.4CoO3-δ perovskite catalysts, and they discovered that a tiny quantity of Sr can make the cobalt nanoparticles extensively dispersed on a carrier composed of metal carbonates and metal oxides and boost the catalytic activity. Additionally, the presence of strontium oxide decreases the production of CO. Ma et al. [13] prepared an LaXCoO3 (X = Mg, Ca, Sr, Ce) perovskite composite catalyst by the citric acid complex method for hydrogen production from ethanol steam. The results showed that Sr-doped samples exhibited excellent activity and stability and showed better catalytic performance than the other samples. Cui et al. [14] pointed out that the catalyst containing Ce has high hydrogen storage capacity, can effectively disperse active metals and inhibit sintering, and Ce can also promote the gasification of carbon substances. The B-site element of perovskite plays an important role in its catalytic performance. Gómez et al. [15] synthesized an La0.8Sr0.2Fe0.8Cr0.2O3 perovskite oxide using a polymerization chemical route, and they demonstrated that La0.8Sr0.2Fe0.8Cr0.2O3 had higher stability and a lower deactivation rate than LaFeO3, as well as better selectivity for hydrogen and methane conversion up to 95%. It demonstrates that the catalyst with the added promoter has better catalytic activity. Natile et al. [16] studied the influence of Co/Fe elements on the physicochemical properties of La0.6Sr0.4Co1-yFeyO3-δ (y = 0.2, 0.5, 0.8) as a methanol/ethanol steam reforming catalyst. They found that the iron element at the B-site can inhibit the formation of by-product CO, especially when the CO/Fe molar ratio is greater than 1. Shen’s research group [17,18] prepared perovskite oxides with different amounts of Co doping by the sol-gel method. The results showed that the doping amount of cobalt at B-site could affect the selectivity of gas phase products through the balance of the water–gas transfer reaction, and the effect of Al2O3 support derived from metal-organic framework on the performance of LaNi0.4Al0.6O3-δ for MSR was studied. The results show that the interaction between the carrier and the active component is strengthened, the dispersion of the active component is improved, the methanol conversion is increased, and the thermal stability is excellent.
Although some studies were conducted on the MSR performance of Lanthanide perovskite, there are few reports using La-Ce-based perovskites as catalysts for MSR. The purpose of this paper is to develop a La-Ce-based perovskite catalyst with high catalytic activity and selectivity for H2 production. Furthermore, the Sr-doping effects, optimal operating conditions for the hydrogen production performance of the synthesized perovskites were investigated in the MSR, which can provide a support for the practical development of the hydrogen energy economy.

2. Results and Discussion

2.1. XRD, SEM and SEM-EDS

The fresh and hydrogen-reduced perovskite La0.6Sr0.4CeO3-δ were examined by XRD to identify the crystalline phase, as shown in Figure 1. It can be seen from the figure that the strong diffraction peak of fresh La0.6Sr0.4CeO3-δ shows the characteristics of the typical perovskite structure as reported in the literature [19], which demonstrates that the lanthanide perovskite-type oxides were successfully synthesized. Generally, the catalysts applied to methanol steam reforming are subjected to pre-reduction treatment. Therefore, the comparison of XRD patterns of La0.6Sr0.4CeO3-δ catalysts before and after reduction by hydrogen can also be seen in Figure 1. The results indicated that the catalyst still maintains the original structure after hydrogen reduction treatment and exhibits a very typical perovskite structure because La0.6Sr0.4CeO3-δ perovskite metal oxides are difficult to reduce with hydrogen. The result is consistent with Shen’s study [18]. The reason for this phenomenon may be that the La0.6Sr0.4CeO3-δ catalyst is a cubic structure [20] and exhibits diffraction corresponding to the cubic perovskite structure (2θ = 32.7°, 37.9° and 54.5°), and some studies have confirmed that the cubic perovskite structure is stable in a reducing environment [21].
In order to more intuitively comprehend the difference in surface morphology between the fresh La0.6Sr0.4CeO3-δ and the reduced La0.6Sr0.4CeO3-δ, the SEM characterization of the two catalysts was carried out, as shown in Figure 2. It can be seen from Figure 2a that the particle size is not uniform, and there were some lumpy particles in the fresh La0.6Sr0.4CeO3-δ sample, showing the characteristics of aggregation. Figure 2b shows the SEM images of La0.6Sr0.4CeO3-δ powders reduced by H2. Compared with the fresh samples, the surface morphological characteristics of the La0.6Sr0.4CeO3-δ catalyst samples after the hydrogen reduction treatment did not change significantly. However, there was a partial reduction in the massive particles, and a certain number of small independent particles appeared that had a more uniform particle distribution and roughly the same particle size, so the activity of the reduced treated catalyst was excellent [22,23].
Energy dispersive X-ray spectroscopy (EDS) was used to analyze the element composition (Figure 3). The correct elemental composition was observed for all characterized samples, and all the elements were uniformly distributed on the catalyst particles. Figure 3a shows the selected area of SEM-EDS mapping, The composition and distribution of each element in the synthesized catalyst material are shown in Figure 3b–e, and all elements are: La, Sr, Ce and O. In addition, the elemental composition of the synthesized catalyst was determined by SEM-EDS. The atomic ratio and nominal atoms of the main elements before and after sample reduction are shown in Table 1. The element ratio of the prepared catalyst sample and the standard element ratio are within the allowable error range, considering the accuracy of SEM-EDS characterization. Therefore, combining the results of EDS and XRD, it can be determined that the perovskite metal oxide catalyst was successfully synthesized. In addition, it can also be seen that the element ratio and standard element ratio of the catalyst sample after reduction are also within the allowable error range, indicating that the perovskite structure has not changed, which is consistent with the XRD results.

2.2. Catalytic Performance

2.2.1. The Effects of A-Site Doping

The composition and ratios of the A/B-site elements of perovskite metal oxides have a great influence on its catalytic activity [24]. The ions on the A-site indirectly promote the catalytic activity. When the A-site ions are replaced, more defects are produced, which affects the electronic state of the B-site ions [25]. A- and B-sites play different roles in the reaction process. B-site mainly affects the temperature range of the reaction, and A-site mainly affects the selectivity of the reaction [26]. In general, Sr was partially substituted for La-site in the perovskite structure to improve the lattice oxygen mobility, which plays a role in the reforming reaction and coke removal [27]. The effect of Sr doping on the catalytic performance of La1-xSrxCeO3-δ (x = 0.2, 0.4, 0.6, 0.8) in MSR was investigated in this study. The MSR performance test results of the catalyst are shown in Figure 4 (the reaction temperature is 600 °C; the molar ratio of water to methanol (W/M) is 3:1; the liquid hourly space velocity (LHSV) is 20 h−1).
As shown in Figure 4a, with the increase in A-site strontium doping amount in perovskite, the methanol conversion first increased and then decreased, among which the strontium doping amount was 0.2 and 0.4, the methanol conversion had no change (approximately 68%); however, when the strontium doping amount was increased to 0.6 or 0.8, the methanol conversion was reduced to 60%. In addition, it was obvious from Figure 4a that strontium doping also showed some influence on hydrogen production. Similar to methanol conversion, hydrogen production displayed a trend of first increasing and then decreasing. La0.6Sr0.4CeO3-δ exhibited the best performance and the maximum hydrogen production per unit time was 3.5 × 10−3 mol/g(cat)/min. As shown in Figure 4b, with the addition of strontium, the gas selectivity of carbon dioxide and carbon monoxide was basically unchanged, indicating that the concentration of strontium at position A had no significant effect on the selectivity of by-products. However, excessive strontium content led to a decrease in H2 selectivity and H2 yield.
In conclusion, considering that methanol conversion and hydrogen production per unit time can best reflect the performance of a methanol steam reforming catalyst, La0.6Sr0.4CeO3-δ exhibited the highest methanol conversion and hydrogen production per unit time, and therefore, it was selected as a candidate for subsequent experiments. Generally, the catalytic performance was also affected by the experimental operating conditions. Therefore, the effects of reforming temperature, W/M and LHSV on MSR were studied.

2.2.2. The Effects of Reforming Temperature

MSR is a strongly endothermic reaction [28], so its catalytic performance is most affected by the reforming temperature. Figure 5 shows the MSR performance of the La0.6Sr0.4CeO3-δ at different reforming temperatures. From Figure 5a, it can be concluded that temperature has a significant effect on methanol conversion and hydrogen production. When the reforming temperature was 500 °C, the methanol conversion and hydrogen production were significantly different from other temperatures. The methanol conversion was less than 10%, and the hydrogen production per unit time was only 0.3 × 10−3 mol/g(cat)/min, probably because MSR is a strong heat-absorbing reaction and low temperature cannot provide enough energy [29]. With the increase in reforming temperature, the methanol conversion (73%) and hydrogen production (3.78 × 10−3 mol/g(cat)/min) reached the maximum at 700 °C. However, when the temperature rises to 800 °C, methanol conversion and hydrogen production per unit time will decrease. The reason was catalyst sintering caused by high temperatures [30]. As shown in Figure 5b, both hydrogen selectivity and hydrogen yield decrease first and then increase with the increase in reforming temperature. However, the selectivity of CO increases first and then decreases. This may be because the methanol decomposition reaction (Equation (2)) requires more energy than the MSR reaction (Equation (1)), so methanol decomposition reaction was inhibited at a low temperature. When the temperature continued to rise, the reverse process of water–gas shift reaction was promoted, thus, increasing the selectivity of CO2. In general, the temperature with the highest methanol conversion and hydrogen production per unit time, 700 °C, was identified as the optimal reforming temperature.

2.2.3. The Effects of the W/M

The hydrogen element in the MSR reaction is partly from water and partly from methanol [31], and the presence of water vapor has a certain impact on the water–gas shift reaction. Therefore, the W/M is also one of the factors affecting the catalytic performance of MSR. In this section, four experiments concerning methanol steam reforming were carried out with the W/M as the research object (the reforming temperature is 700 °C; the LHSV is 20 h−1). The influence of different W/M on catalytic performance is shown in Figure 6. As shown in Figure 6a, when the molar ratio of water to methanol was 2:1, 4:1, 5:1, there was no significant difference in methanol conversion, but when W/M was 3:1, methanol conversion reached the maximum value, and hydrogen production showed a decreasing trend. In addition, a smaller W/M meant that more methanol was needed, and the methanol conversion decreased at the same time, which leads to waste of methanol and increased cost. Figure 6b indicates that the high W/M can suppress the CO selectivity, which may be related to the water–gas shift reaction. The high W/M promoted the reverse process of the WGSR reaction, as shown in Equation (3). However, considering that methanol conversion and hydrogen production can best reflect the catalyst performance of methanol steam reforming, the best water-to-methanol molar ratio for the next experiment was determined to be W/M of 3:1.

2.2.4. The Effects of the LHSV

The liquid hourly space velocity (LHSV) was also one of the factors affecting the performance of methanol steam reforming. The liquid refers to methanol and water. In order to explore the influence of LHSV on the performance of reforming reaction, MSR experiments were carried out at 10 h−1, 15 h−1, 20 h−1 and 25 h−1, respectively, (reforming temperature is 700 °C; W/M is 3:1). The experimental results were shown in Figure 7. The influence of different LHSV on the catalytic activity of the catalyst and the selectivity/yield of gas products are shown in Figure 7a,b, respectively. It can be seen from Figure 7a that methanol conversion reaches the maximum value of 82% at LHSV of 20 h−1, while hydrogen production increases with the increase in LHSV. However, LHSV should not be too high, because too high airspeed will lead to a decline in the methanol conversion rate, resulting in waste of methanol. It can be seen from Figure 7b that the LHSV has small influence on the selectivity of gas products and the yield of hydrogen. Furthermore, the trend of hydrogen selectivity was similar to that of hydrogen yield, both of which were decreasing first and then increasing. In addition, the selectivity of CO decreased first and then increased, while the selectivity of CO2 exhibits the opposite trend. In summary, the reforming temperature of 700 °C, the W/M of 3:1 and the LHSV of 20 h−1 were the optimal experimental conditions for perovskite oxide La0.6Sr0.4CeO3-δ in MSR.

3. Materials and Methods

3.1. Preparation of La1-xSrxCeO3-δ Perovskite Powders

The perovskite-type metal oxide catalyst was prepared by the sol-gel method with citric acid as a complexing agent and ethylenediaminetetraacetic EDTA acid as an auxiliary complexing agent. La (NO3)3·6H2O (99%), Sr (NO3)2 (99%) and Ce (NO3)2·6H2O (99%) were applied as the raw materials for metal precursors, which were obtained from the Aladdin Corporation. For preparing 0.02 mol perovskite powder as an example, first, the required metal precursors were weighed, added to approximately 120 mL of deionized water and stirred to dissolve. Then, the precursor solution was supplemented with a certain proportion of citric acid and ethylenediaminetetraacetic acid while being stirred, and the molar ratio of metal nitrate, citric acid and EDTA was 1:1.5:1 [32]. The resulting mixture was stirred in a water bath at 80 °C for 4–5 h to obtain the gel. The gel was then dried for 12 h at 110 °C in a drying oven to obtain a fluffy structured substance. The resulting fluffy substance was milled into a powder and put in a muffle furnace to calcine for 30 min at 400 °C and then for 7 h at 850 °C. The purpose of calcination was to remove organic compounds [33]. Finally, the calcined material was ground to obtain the final perovskite catalyst.

3.2. Characterization

The samples were characterized by X-ray diffraction (D/MAX-Ultima+ diffractometer), and the phase composition of the samples was determined with a Co-Kα monochromatic X-ray source (1.7902 Å, 40 kV, 40 mA). The diffraction patterns in the range of 2θ of 10–90° were recorded with a scanning step of 0.02°. The surface morphology (SEM) and chemical composition (EDS) of the synthesized samples was analyzed by scanning electron microscopy (SUPRA 55 SAPPHIRE, ZEISS, Jena, Germany).

3.3. Methanol Steam Reforming Experiments

The synthesized perovskite catalyst sample was used in the MSR reaction for hydrogen production. First, 0.3 g of catalyst was weighed and placed into the middle of a quartz tube, where the reaction temperature was controlled by a thermocouple in the tube furnace. The mass flow controller was responsible for regulating the gas flow rate in the MSR experiment.
The temperature of the reactor was first heated from room temperature to 300 °C while being purged with 30 mL/min of nitrogen. The temperature was then raised to 600 °C and the catalyst sample was reduced under a mixture gas of 10%H2–90%N2 for 40 min. Following this, the experimental system was purged with N2 at a catalytic temperature. The configured mixed solution of water and methanol was mounted on a micro-pump and pumped to the steam generator at 130 °C according to the preset feed flow rate, where it turned into steam, and subsequently, the methanol water vapor was brought into the reactor at 30 mL/min N2. The volume concentrations of H2, CO and CO2 were recorded with an on-line gas analyzer, and methanol conversion, the H2 yield, the selectivity of gas products and hydrogen production per unit time were calculated as follows:
X m e t h a n o l = ( 1 n m e t h a n o l o u t n m e t h a n o l i n ) × 100 %
Y H 2 = F H 2 n m e t h a n o l i n
S H 2 = F H 2 ( n m e t h a n o l i n n m e t h a n o l o u t ) × 3 × 100 %
S i = F i F C O + F C O 2 + F H 2 × 100 %
P H 2 = C H 2 × f p r o d u c t s m c a t × 10 6
where Xmethanol (%), Y H 2 (mol/mol methanol), S H 2 (%), Si (%, i = CO, CO2) and P H 2 (mol/g(cat)/min) were the CH3OH conversion, H2 yield, H2 selectivity, the CO/CO2 selectivity and hydrogen production of 1 g catalyst, respectively. More information on the parameter annotations in the equations was provided in the previous literature [17].

4. Conclusions

La1-xSrxCeO3-δ (x = 0.2, 0.4, 0.6, 0.8) perovskite powders were synthesized by the sol-gel method and applied for MSR to produce H2. The effect of Sr doping and the reaction conditions of La0.6Sr0.4CeO3-δ perovskite powders were studied in-depth by characterization with SEM, XRD, EDS and the MSR experiments. The main conclusions are as follows:
  • The experimental results showed that La0.6Sr0.4CeO3-δ has the highest methanol conversion and hydrogen production per unit time among the La1-xSrxCeO3-δ. In addition, excessive Sr content led to a decrease in H2 selectivity and H2 yield.
  • The results of XRD and SEM-EDS showed that the La0.6Sr0.4CeO3-δ catalyst was successfully synthesized in this study. The catalyst still maintains the original structure after hydrogen reduction treatment and exhibits a very typical perovskite structure because La0.6Sr0.4CeO3-δ perovskite metal oxides are difficult to reduce with hydrogen. The reason for this phenomenon may be that the La0.6Sr0.4CeO3-δ catalyst is a cubic structure, and some studies have confirmed that the cubic perovskite structure is stable in a reducing environment. The results of SEM indicated that the surface morphology of the catalyst sample after reduction treatment did not change significantly compared with that of the fresh sample. The reduced catalyst sample has more uniform particle distribution and roughly the same particle size, so the catalyst activity is more excellent.
  • The influence of experimental conditions on the catalytic performance of La0.6Sr0.4CeO3-δ catalyst was investigated in this study, and the optimal reforming temperature, W/M and LHSV were determined to be 700 °C, 3:1 and 20 h−1, respectively. The maximum methanol conversion rate was 82%, and the hydrogen production per unit time could reach 3.2 × 10−3 mol/g(cat)/min. La0.6Sr0.4CeO3-δ is a potential catalyst for methanol steam reforming with good catalytic performance. The potential of methanol to hydrogen depends on the catalyst with high selectivity for hydrogen at low temperatures. Therefore, the steam reforming of methane over the Sr-doped LaCeO3-δ catalyst shows good promise for the development of an efficient, economical and clean hydrogen production system.

Author Contributions

Conceptualization, Q.S.; methodology, Z.C.; software, Z.S.; formal analysis, S.L.; writing—original draft preparation, G.C.; writing—review and editing, Q.S.; data curation, X.Z.; supervision, G.Y. All authors have read and agreed to the published version of the manuscript.

Funding

This work was supported by China Postdoctoral Science Foundation (No.2019M651094) and Science and Technology Innovation Foundation of Dalian (2021JJ11CG004).

Institutional Review Board Statement

Not applicable.

Informed Consent Statement

Not applicable.

Data Availability Statement

Not applicable.

Conflicts of Interest

The authors declare no conflict of interest.

References

  1. Chiu, M.; Kuo, C.; Huang, C.; Yang, W. Preparation of CuS/PbS/ZnO Heterojunction Photocatalyst for Application in Hydrogen Production. Catalysts 2022, 12, 1677. [Google Scholar] [CrossRef]
  2. Anandarajah, G.; McDowall, W.; Ekins, P. Decarbonising road transport with hydrogen and electricity: Long term global technology learning scenarios. Int. J. Hydrog. Energy 2013, 38, 3419–3432. [Google Scholar] [CrossRef]
  3. Dutta, S. A review on production, storage of hydrogen and its utilization as an energy resource. J. Ind. Eng. Chem. 2014, 20, 1148–1156. [Google Scholar] [CrossRef]
  4. Cheng, Z.; Zhou, W.; Lan, G.; Sun, X.; Wang, X.; Jiang, C.; Li, Y. High-performance Cu/ZnO/Al2O3 catalysts for methanol steam reforming with enhanced Cu-ZnO synergy effect via magnesium assisted strategy. J. Energy Chem. 2021, 63, 550–557. [Google Scholar] [CrossRef]
  5. Aramouni, N.A.K.; Touma, J.G.; Tarboush, B.A.; Zeaiter, J.; Ahmad, M.N. Catalyst design for dry reforming of methane: Analysis review. Renew. Sustain. Energy Rev. 2018, 82, 2570–2585. [Google Scholar] [CrossRef]
  6. Shen, Q.; Cai, Z.; Shao, Z.; Yang, G.; Li, S. Improved performance of bimetallic oxides CuO-Y2O3 synthesized by sol-gel for methanol steam reforming. J. Am. Ceram. Soc. 2022, 105, 6839–6850. [Google Scholar] [CrossRef]
  7. Mosinska, M.; Stępińska, N.; Maniukiewicz, W.; Rogowski, J.; Mierczynska-Vasilev, A.; Vasilev, K.; Mierczynski, P. Hydrogen Production on Cu-Ni Catalysts via the Oxy-Steam Reforming of Methanol. Catalysts 2020, 10, 273. [Google Scholar] [CrossRef] [Green Version]
  8. Nilsson, M.; Jozsa, P.; Pettersson, L.J. Evaluation of Pd-based catalysts and the influence of operating conditions for autothermal reforming of dimethyl ether. Appl. Catal. B: Environ. 2007, 76, 42–50. [Google Scholar] [CrossRef]
  9. Vidal Vázquez, F.; Simell, P.; Pennanen, J.; Lehtonen, J. Reactor design and catalysts testing for hydrogen production by methanol steam reforming for fuel cells applications. Int. J. Hydrog. Energy 2016, 41, 924–935. [Google Scholar] [CrossRef]
  10. Wu, G.; Li, S.; Zhang, C.; Wang, T.; Gong, J. Glycerol steam reforming over perovskite-derived nickel-based catalysts. Appl. Catal. B: Environ. 2014, 144, 277–285. [Google Scholar] [CrossRef]
  11. Zhang, Y.; Guo, L.; Xu, Q.; Zhang, Q.; Li, J.; Ma, Q. Effect of Sr-Doping on the Photocatalytic Performance of LaNiO3−σ. Catalysts 2022, 12, 1434. [Google Scholar] [CrossRef]
  12. Morales, M.; Segarra, M. Steam reforming and oxidative steam reforming of ethanol over La0.6Sr0.4CoO3−δ perovskite as catalyst precursor for hydrogen production. Appl. Catal. A Gen. 2015, 502, 305–311. [Google Scholar] [CrossRef]
  13. Ma, F.; Ding, Z.; Chu, W.; Hao, S.; Qi, T. Preparation of LaXCoO3 (X = Mg, Ca, Sr, Ce) catalysts and their performance for steam reforming of ethanol to hydrogen. Chin. J. Catal. 2014, 35, 1768–1774. [Google Scholar] [CrossRef]
  14. Cui, Y.; Galvita, V.; Rihko-Struckmann, L.; Lorenz, H.; Sundmacher, K. Steam reforming of glycerol: The experimental activity of La1−xCexNiO3 catalyst in comparison to the thermodynamic reaction equilibrium. Appl. Catal. B: Environ. 2009, 90, 29–37. [Google Scholar] [CrossRef]
  15. Gómez-Cuaspud, J.A.; Perez, C.A.; Schmal, M. Nanostructured La0.8Sr0.2Fe0.8Cr0.2O3 Perovskite for the Steam Methane Reforming. Catal. Lett. 2016, 146, 2504–2515. [Google Scholar] [CrossRef]
  16. Natile, M.M.; Poletto, F.; Galenda, A.; Glisenti, A.; Montini, T.; Rogatis, L.D.; Fornasiero, P. La0.6Sr0.4Co1-yFeyO 3-δ perovskites: Influence of the Co/Fe atomic ratio on properties and catalytic activity toward alcohol steam-reforming. Chem. Mater. 2008, 20, 2314–2327. [Google Scholar] [CrossRef]
  17. Shao, Z.; Shen, Q.; Ding, H.; Jiang, Y.; Li, S.; Yang, G. Synthesis, characterization, and methanol steam reforming performance for hydrogen production on perovskite-type oxides SrCo1-xCuxO3-δ. Ceram Int. 2022, 48, 11836–11848. [Google Scholar] [CrossRef]
  18. Shen, Q.; Shao, Z.; Cai, Z.; Yan, M.; Yang, G.; Li, S. Enhancement of hydrogen production performance of novel perovskite LaNi0.4Al0.6O3-δ supported on MOF A520-derived λ-Al2O3. Int. J. Energy Res. 2022, 46, 15709–15721. [Google Scholar] [CrossRef]
  19. Shen, Q.; Li, S.; Yang, G.; Yuan, J.; Huang, N. Development of microwave-assisted sol-gel rapid synthesis of nano-crystalline perovskites oxygen carrier material in oxyfuel combustion. J. Ceram. Process. Res. 2019, 20, 152–157. [Google Scholar] [CrossRef]
  20. Mangu, S.; Suares, V.; Gupta, A.; Anantharaman, A.P. Synthesis, characterization and density Functional theory (DFT) study of LaCeO3. Mater. Today: Proc. 2022, 57, 1892–1897. [Google Scholar] [CrossRef]
  21. Jangam, A.; Das, S.; Pati, S.; Kawi, S. Catalytic reforming of tar model compound over La1-xSrx-Co0.5Ti0.5O3-δ dual perovskite catalysts: Resistance to sulfide and chloride compounds. Appl. Catal. A: Gen. 2021, 613, 118013. [Google Scholar] [CrossRef]
  22. Xu, X.; Shuai, K.; Xu, B. Review on Copper and Palladium Based Catalysts for Methanol Steam Reforming to Produce Hydrogen. Catalysts 2017, 7, 183. [Google Scholar] [CrossRef]
  23. Luan, X.; Qi, L.; Zheng, Z.; Gao, Y.; Xue, Y.; Li, Y. Step by Step Induced Growth of Zinc-Metal Interface on Graphdiyne for Aqueous Zinc-Ion Batteries. Angew. Chem. Int. Ed. 2023. [Google Scholar] [CrossRef]
  24. Shen, Q.; Li, S.; Yang, G.; Sunden, B.; Yuan, J. Effect of A-/B-site Doping on Oxygen Non-Stoichiometry, Structure characteristics, and O2 Releasing Behavior of La1−xCaxCo1−yFeyO3−δ Perovskites. Energies 2019, 12, 410. [Google Scholar] [CrossRef] [Green Version]
  25. Yang, P.; Li, N.; Teng, J.; Wu, J.; Ma, H. Influence of A-site cation in La0.7M0.3Ni0.7Fe0.3O3 (M = Pr, Y, Sr, Zr, Ce) perovskite-type oxides on the catalytic performance. Chem. Res. Appl. 2018, 30, 1979–1985. [Google Scholar]
  26. Shen, Q.; Dong, S.; Li, S.; Yang, G.; Pan, X. A Review on the Catalytic Decomposition of NO by Perovskite-Type Oxides. Catalysts 2021, 11, 622. [Google Scholar] [CrossRef]
  27. Mukai, D.; Izutsu, Y.; Sekine, Y. Highly and stably dispersed Pt catalysts supported over La1−xSrxAlO3−0.5x perovskite for oxidative methane activation and their structures. Appl. Catal. A Gen. 2013, 458, 71–81. [Google Scholar] [CrossRef]
  28. Da Silva Veras, T.; Mozer, T.S.; da Costa Rubim Messeder dos Santos, D.; da Silva César, A. Hydrogen: Trends, production and characterization of the main process worldwide. Int. J. Hydrog. Energy 2017, 42, 2018–2033. [Google Scholar] [CrossRef]
  29. Yang, E.; Noh, Y.; Hong, G.; Moon, D. Combined steam and CO2 reforming of methane over La1-xSrxNiO3 perovskite oxides. Catal. Today 2018, 299, 242–250. [Google Scholar] [CrossRef]
  30. Shen, Q.; Zheng, Y.; Luo, C.; Ding, N.; Zheng, C.; Thern, M. Effect of A/B-site substitution on oxygen production performance of strontium cobalt based perovskites for CO2 capture application. RSC Adv. 2015, 5, 39785–39790. [Google Scholar] [CrossRef]
  31. Abdalla, A.M.; Hossain, S.; Nisfindy, O.B.; Azad, A.T.; Dawood, M.; Azad, A.K. Hydrogen production, storage, transportation and key challenges with applications: A review. Energy Convers. Manag. 2018, 165, 602–627. [Google Scholar] [CrossRef]
  32. Shen, Q.; Jiang, Y.; Li, S.; Yang, G.; Zhang, H.; Zhang, Z.; Pan, X. Hydrogen production by ethanol steam reforming over Ni-doped LaNixCo1−xO3−δ perovskites prepared by EDTA-citric acid sol–gel method. J. Sol-Gel Sci. Technol. 2021, 99, 420–429. [Google Scholar] [CrossRef]
  33. Ding, H.; Xu, Y.; Luo, C.; Wang, Q.; Li, S.; Cai, G.; Zhnag, L.; Zhang, Y.; Shen, Q. Oxygen desorption behavior of sol-gel derived perovskite-type oxides in a pressurized fixed bed reactor. Chem Eng. J. 2017, 323, 340–346. [Google Scholar] [CrossRef]
Figure 1. XRD pattern of La0.6Sr0.4CeO3-δ catalysts before and after reduction by hydrogen.
Figure 1. XRD pattern of La0.6Sr0.4CeO3-δ catalysts before and after reduction by hydrogen.
Catalysts 13 00248 g001
Figure 2. SEM images of (a) the fresh La0.6Sr0.4CeO3-δ sample, (b) the La0.6Sr0.4CeO3-δ sample after reduction treatment.
Figure 2. SEM images of (a) the fresh La0.6Sr0.4CeO3-δ sample, (b) the La0.6Sr0.4CeO3-δ sample after reduction treatment.
Catalysts 13 00248 g002
Figure 3. SEM-EDS mapping images of the fresh La0.6Sr0.4CeO3-δ: (a) the selected area of SEM-EDS mapping; (b) lanthanum; (c) strontium; (d) cerium; (e) oxygen.
Figure 3. SEM-EDS mapping images of the fresh La0.6Sr0.4CeO3-δ: (a) the selected area of SEM-EDS mapping; (b) lanthanum; (c) strontium; (d) cerium; (e) oxygen.
Catalysts 13 00248 g003aCatalysts 13 00248 g003b
Figure 4. The MSR catalytic performance of the La1-xSrxCeO3-δ (x = 0.2, 0.4, 0.6, 0.8): (a) methanol conversion (left Y) and hydrogen production of 1g catalyst (right Y); (b) gas selectivity (left Y) and hydrogen yield (right Y).
Figure 4. The MSR catalytic performance of the La1-xSrxCeO3-δ (x = 0.2, 0.4, 0.6, 0.8): (a) methanol conversion (left Y) and hydrogen production of 1g catalyst (right Y); (b) gas selectivity (left Y) and hydrogen yield (right Y).
Catalysts 13 00248 g004
Figure 5. The MSR performance of the La0.6Sr0.4CeO3-δ at different reforming temperatures: (a) methanol conversion (left Y) and hydrogen production of 1 g catalyst (right Y); (b) gas selectivity (left Y) and hydrogen yield (right Y).
Figure 5. The MSR performance of the La0.6Sr0.4CeO3-δ at different reforming temperatures: (a) methanol conversion (left Y) and hydrogen production of 1 g catalyst (right Y); (b) gas selectivity (left Y) and hydrogen yield (right Y).
Catalysts 13 00248 g005
Figure 6. The MSR performance of the La0.6Sr0.4CeO3-δ at different W/M: (a) methanol conversion (left Y) and hydrogen production of 1g catalyst (right Y); (b) gas selectivity (left Y) and hydrogen yield (right Y).
Figure 6. The MSR performance of the La0.6Sr0.4CeO3-δ at different W/M: (a) methanol conversion (left Y) and hydrogen production of 1g catalyst (right Y); (b) gas selectivity (left Y) and hydrogen yield (right Y).
Catalysts 13 00248 g006
Figure 7. The MSR performance of the La0.6Sr0.4CeO3-δ at different LHSV: (a) methanol conversion (left Y) and hydrogen production of 1 g catalyst (right Y); (b) gas selectivity (left Y) and hydrogen yield (right Y).
Figure 7. The MSR performance of the La0.6Sr0.4CeO3-δ at different LHSV: (a) methanol conversion (left Y) and hydrogen production of 1 g catalyst (right Y); (b) gas selectivity (left Y) and hydrogen yield (right Y).
Catalysts 13 00248 g007
Table 1. The SEM-EDS data of the La0.6Sr0.4CeO3-δ sample.
Table 1. The SEM-EDS data of the La0.6Sr0.4CeO3-δ sample.
ElementsStandard Atomic RatioAtomic Ratio of the Fresh La0.6Sr0.4CeO3-δAtomic Ratio of the La0.6Sr0.4CeO3-δ Reduced by H2
La98.763.64
Sr65.871.82
Ce1515.106.33
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content.

Share and Cite

MDPI and ACS Style

Chen, G.; Shen, Q.; Zhang, X.; Cai, Z.; Shao, Z.; Li, S.; Yang, G. Methanol Steam Reforming over La1-xSrxCeO3-δ Catalysts for Hydrogen Production: Optimization of Operating Parameters. Catalysts 2023, 13, 248. https://doi.org/10.3390/catal13020248

AMA Style

Chen G, Shen Q, Zhang X, Cai Z, Shao Z, Li S, Yang G. Methanol Steam Reforming over La1-xSrxCeO3-δ Catalysts for Hydrogen Production: Optimization of Operating Parameters. Catalysts. 2023; 13(2):248. https://doi.org/10.3390/catal13020248

Chicago/Turabian Style

Chen, Gaokui, Qiuwan Shen, Xin Zhang, Zhongwen Cai, Zicheng Shao, Shian Li, and Guogang Yang. 2023. "Methanol Steam Reforming over La1-xSrxCeO3-δ Catalysts for Hydrogen Production: Optimization of Operating Parameters" Catalysts 13, no. 2: 248. https://doi.org/10.3390/catal13020248

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.