Unlocking the Potential of N-Doped SnO2 for Sustainable Photocatalytic Degradation of Carcinogenic Dyes

1
Department of Chemistry, University of Delhi, Delhi 110007, India
2
Department of Biochemistry, University of Delhi, Delhi 110007, India
3
Department of Chemistry, Gurukula Kangri (Deemed to Be University), Haridwar 249404, India
4
Department of Chemistry, Shivaji College, University of Delhi, Delhi 110021, India
5
Department of Bioscience, Himachal Pradesh University, Shimla 171005, India
6
Department of Chemistry, Durban University of Technology, Steve Biko Road, Durban 4001, South Africa
7
Department of Chemical and Metallurgical, Vaal University of Technology, Vanderbijlpark 1900, South Africa
8
Academy of Nanotechnology and Waste Water Innovations, Johannesburg 2007, South Africa
9
Special Centre for Nano Science, Jawaharlal Nehru University, Delhi 110067, India
*
Authors to whom correspondence should be addressed.
Separations 2023, 10(6), 322; https://doi.org/10.3390/separations10060322
Submission received: 26 April 2023 / Revised: 12 May 2023 / Accepted: 19 May 2023 / Published: 23 May 2023

Abstract

:
Environmental adulteration is an emerging concern due to the discharge of wastewater effluents from several sources. Several carcinogenic dyes are the major contaminants in these water bodies. These could cause long-lasting and detrimental effects to humans as well as aquatic ecosystems. For efficient degradation of such dyes, the exploration of nanotechnology has demonstrated huge potential. Herein, the degradation of dyes (MB, CV, and MO) has been carried out photocatalytically using N-doped SnO2 nanoparticles (N:SnO2 NPs) as well as in presence of a sacrificial agent, EDTA. These NPs were synthesized at an ambient temperature. Different characterization techniques were used throughout the analysis of the synthesized NPs. The PXRD analysis reveals formation of single-phase rutile structure with tetragonal symmetry. Using the Scherrer formula, the size of the NPs was found to be less than 5 nm, exhibiting increases in size with N doping. Further, morphological analysis through field emission scanning electron microscopy (FESEM) and transmission electron microscopy (TEM) examined the existence of highly agglomerated, spherical NPs. The thermogravimetric analysis (TGA) results depict the thermal stability of the synthesized NPs up to a temperature of 800 °C. These synthesized N:SnO2 NPs exhibit potent efficiency for the photocatalytic degradation of MB, MO, and CV dyes with an efficiency of 93%, 83%, and 73% degradation, respectively, under UV light irradiation. Additionally, the effect of the sacrificial agent, EDTA, was observed on the degradation process and resulted in a degradation of ~90% MB dye, 88% CV dye, and 86% MO dye within 15 min of UV light irradiation.

1. Introduction

Rapid industrialization and increasing urbanization in the 21st century are emerging concerns regarding environmental pollution [1]. For researchers and professionals working in the field of environmental pollutants and especially water contaminants, the critical challenge lies in effectively removing wastewater that contains carcinogenic effluents from ground water [2,3]. Adjacently, wastewater purification with conventional methods is leading to an energy crisis across the globe. Current advancements in science opt for newer chemicals to be used in various industries, and these are organic dyes which are used in a number of industries, such as the fabric and leather industries [3,4,5]. Compared to other contaminants present in water, dyes have been recognized as the most easily recognizable pollutants owing to their color visibility in ever lower concentrations of 1 ppm [6]. It has been reported that industrial dying stuffs are the major contributors of toxic organic pollutants contaminating water [7]. Acidic and reactive dyes, being water soluble, are the most difficult to handle. Reactive dyes are rarely preferred for the dying of fabrication, owing to the problem that the remaining effluent is directly discharged into the water [8]. When these dyes are not ionized into water, they tend to bioaccumulate with aquatic life [9]. The main concern with dye effluents is their synthesis using carcinogenic aromatic compounds. The literature proposes a number of methods adopted for water purification that are associated with one or more limitation [2,10,11]. Taking the very simple and easiest method of adsorption, the adsorbent still carries the adsorbate on its surface, and hence needs to be disposed of again, leading to pollution [12]. Here, in this work, one of the most efficient processes has been used for the elimination of carcinogenic dyes from water: photocatalysis [13]. This method produces no secondary contaminants but itself degrades the primary contaminants into less toxic substances [14].
The elimination of carcinogenic dyes from water has been the subject of numerous investigations in the literature. After conducting a thorough literature survey, it was found that while there were few articles related to the synthesis of N-doped SnO2 nanoparticles (N:SnO2 NPs) and their characterization, there is a lack of literature available for removing dyes from water. However, a number of SnO2-based nanocomposites have been reported for photocatalytic dye degradation. Xu et al. compared the photocatalytic degradation of RhB dye with TiO2, SnO2, N-TiO2, and N-TiO2/SnO2 and explained that the highest degradation was observed with N-TiO2/SnO2. The composite completely degraded the dye within 300 min of light irradiation [15,16]. Chen et al. used hydrothermally synthesized quantum dots modified with a N:SnO2 composite to degrade RhB dye. It enhances the performance from 20% to 99% for RhB dye compared to pure SnO2 within 120 min [17]. N:SnO2 nano-powder crystals were produced by Liu et al. via a solid-phase reaction technique that involved the utilizing of a surfactant, i.e., sodium p-toluene sulfonate (STS), and the process was performed at room temperature. The results showed enhanced degradation capacity of rice straw powder treatment wastewater (RSPTW), which occurs due to the formation of free radicals because of a low calcination temperature [18]. These studies demonstrate the potential of N:SnO2 NPs as photocatalysts for dye degradation, and suggest that further research on N:SnO2 NPs could lead to the development of more efficient and effective methods for the elimination of aqueous dyes.
Furthermore, the previously synthesized N:SnO2 NPs via a novel solution-based method have been reported for their application in dihydrogen production. To explore other possibilities, the photocatalytic performance of the N:SnO2 NPs for dye degradation has been studied in the present work. Given the preceding discussion, it was thought worthwhile to investigate the potential of N:SnO2 NPs in photocatalytic dye degradation. N:SnO2 NPs offer immense utilization among various domains, especially in the context of sustainable sources. Hence, in this work, a facile and novel solution-based synthesis of N:SnO2 NPs at room temperature was carried out as previously described by Bhawna et al. [19]. These NPs have been explored as efficient photocatalysts for the decomposition of methylene blue (MB), methyl orange (MO), and crystal violet (CV) dyes when exposed to UV light.
Overall, this research could open up new avenues for environmental-associated concerns by providing an efficient and sustainable method for the degradation of carcinogenic dyes from water. The use of N:SnO2 NPs as photocatalysts offers a potential solution to the environment problems associated with water pollution caused by industrial dyes. Moreover, the synthesis of N:SnO2 NPs at room temperature through the simple and efficient solution-based method described in our study offers immense potential for various sustainable applications beyond the realm of dye degradation. For instance, these NPs could be utilized as a photocatalyst for hydrogen production, as previously reported by Bhawna et al. [19]. The use of sustainable materials and processes is crucial for addressing environmental challenges, and the development of such technologies can have far-reaching implications for industries and communities worldwide.
In the future, this research can pave the way for the development of more efficient and environmentally sustainable methods to manage wastewater and other forms of environmental industrialization, which have become pressing concerns in the present century. Our research output can encourage further exploration and innovation in the field of sustainable environmental solutions.

2. Experimental

2.1. Materials and Methods

All chemicals were of a high purity >99.9%; SnCl2•2H2O (tin (II) chloride dihydrate; Merck Chemicals, Rahway, NJ, USA), CH3OH (methanol; Merck Chemicals, Rahway, NJ, USA), H2O2 (hydrogen peroxide; Qualigens, Thermo Fisher Scientific India Pvt. Ltd., Maharashtra, India).

2.2. Synthesis of N-Doped SnO2 Nanoparticles

The N:SnO2 NPs were prepared as described by Bhawna et al. [19]. In brief, a 0.5 M SnCl2•2H2O (Merck) solution was prepared in methanol and was diluted with 60 mL of methanol. Further, it was continuously stirred with 40 mL of hydrazine hydrate (Fisher Scientific Ltd., Waltham, MA, USA) and left at room temperature for 4 h. The pale, yellow-colored substance was then centrifuged, washed in methanol, and dried at 60 °C.

2.3. Characterization Studies

The powder X-ray diffraction (PXRD) patterns of the prepared N:SnO2 NPs were carried out using a high-resolution D8 Discover Bruker X-ray diffractometer with radiation of Cu Kα at wavelength 1.5418 Å; the operating voltage is 40 kV, and the 15 mA current is applied. The prepared sample was coated onto the glass substrate, and the XRD patterns were recorded at 2θ from 5° to 80° with a scanning speed of 1°/min and scanning steps of 0.02°/min. The morphology of the N:SnO2 NPs were demonstrated using a Zeiss GeminiSEM 500 Thermal field emission-type FESEM with a scanning voltage of 0.02–30 kV. Moreover, to gather a detailed understanding of the N:SnO2 NPs, transmission electron microscopy (TEM) using TEM-JEOL 2100F was carried out. Thermogravimetric analysis (TGA) was also performed on HiRes1000 RT up to 1100C to determine the thermal stability with a continuous flow of nitrogen at a heating rate of 10 °C/min.

2.4. Photocatalytic Dye Degradation Performance

The photocatalytic performance of the N:SnO2 NPs was evaluated in terms of degradation of MB, MO, and CV dyes when exposed to UV light and also in the presence of EDTA as a sacrificial agent. The reaction beaker was positioned on a magnetic stirrer, which had an aperture at the top for the purpose of exposure to UV light irradiation. Briefly, a quantity of 0.1 g of catalyst was added to 100 mL of dye solution with a concentration of 20 × 10−6 M. In total, 10 mL of the reference standard was centrifuged and collected. The solution was stirred continuously for 30 min under dark conditions to ensure that an adsorption–desorption equilibrium between the dye and the catalyst was reached. After dark reaction, 10 mL of the solution was centrifuged and collected. The UV light lamp was switched on for the light reaction. Subsequently, the solution was exposed to UV light. At 15 min intervals, a specific volume of 10 mL of the sample was taken and centrifuged, and the concentration of the sample was measured using UV-Vis spectroscopy. Similar steps were followed with the CV and MO dyes. The experiments were also performed by adding a drop of 3 mM EDTA into the dye solution to observe the effect of the sacrificial agent on the degradation process. The rate of MB, MO, and CV dye degradation under UV light radiation as well as the absorbance of the collected samples was measured at λmax, and the degradation rate was calculated using the following formula:
Dye   degradation   efficiency   % = C 0 C t C 0 × 100
where C0 represents the initial concentration and Ct represents the final concentration at time t. The term “time” (t) refers to the amount of time needed for the catalyst to degrade 50% of the dye in an aqueous solution.

3. Results and Discussion

3.1. Powder XRD Analysis

Figure 1 illustrates the diffraction pattern of the N:SnO2 NPs fabricated via a facile chemical approach at room temperature. The figure demonstrates the rutile structure of the nanoparticles, with crystal lattice parameters presented in Table S1, along with space group P42/mnm and tetragonal symmetry. The diffraction peaks at different theta (2θ) values demonstrate a clear mirroring of the crystallographic planes (110), (101), (200), (211), (220), (002), (310), and (221), respectively. Further, this corresponds to JCPDS file number 41-1445 [20,21,22,23,24,25]. Apart from the abovementioned diffraction peaks, no other intense peak was observed, thus indicating the high purity of the N:SnO2 NPs. Additionally, it can be elucidated that the observed diffraction peaks overlap the standard characteristic peak positions of the SnO2 NPs, which confirms a single-phase synthesis of the desired N:SnO2 NPs prepared using the solution-based synthesis.
The Scherrer formula was used to determine the average crystalline size of the N:SnO2 NPs, as shown below:
D = k λ β c o s θ
where D represents the crystallite size, k is a constant equivalent to 0.9, λ is the wavelength of the X-ray, β is the full width at half maximum (FWHM), and θ is Bragg’s diffraction angle. The diffraction that was picked to calculate the crystalline size is the intensity peak at d211. From this, the calculated size of the crystallite was found to be 3.4 nm, whilst the crystalline size of the pure SnO2 NPs was found to be 0.6 nm. Therefore, the size of the crystallite illustrates that the size of the N:SnO2 increases with the doping of N.
The Williamson–Hall (W–H) method is a popularly used approach to evaluate the lattice strain and the crystalline size of the desired material. It does so by investigating the broadness of the PXRD peaks that occurs due to intrinsic strain. As it takes into account the microstrain as well as the crystalline size of the material, it is thus beneficial for interpreting the overall broadening of the XRD peak [26,27]. The equation used to calculate the W–H plot using the following equation is as follows:
β T o t a l = β S t r a i n + β C r y s t a l l i n e   S i z e
Herein, β S t r a i n   = ε × 4 t a n θ and β C r y s t a l l i n e   S i z e = k λ D c o s θ . Therefore, upon substituting βstrain and βcrystalline size to the above equation:
β T o t a l = ε × 4 t a n θ + k λ D   c o s θ
β T o t a l × c o s θ = ε × 4 s i n θ + k λ D  
where, ε represents the intrinsic strain and λ is the wavelength of the X-ray beam, i.e., equivalent to 0.154 nm. After performing the linear fitting, the W–H plot is illustrated in Figure 2.
From the graph, the intrinsic strain and average size of the crystallite was enumerated to be approximately −7.56 × 10−3 and 4.3 nm, respectively. The expansion of the lattice overserved in the W–H plot can be attributed to an increase in the size of the crystalline structure in the N:SnO2 NPs, as indicated by the negative slope. This confinement can cause the atoms within the crystal to be arranged differently than they would be in their bulk counterpart, resulting in lattice expansion [19].

3.2. Morphological Analysis

The morphological identification of N:SnO2 NPs was exhibited via FESEM analysis (Figure 3) and TEM (Figure 4). FESEM imaging reveals the formation of uniformly distributed spherical NPs. However, there is high agglomeration of the NPs, which is common in NM synthesis. As can be seen from Figure 3A, the distribution of the particles is completely uniform. The corresponding micrographs for elemental mapping of the NPs are shown in Figure 3C. The distribution of elements in the mapping micrographs has been demonstrated with different colors, such as yellow, representing Sn, red for N, and green for O. The elemental distribution in the mapping micrographs endorses the formation of N:SnO2 NPs. In our previous report, the concentration of N ions incorporated into the tin lattice using X-ray photoelectron spectroscopy (XPS) was found to be 4.6% [19].
Additionally, the TEM image provides a detailed view of the morphology of the synthesized NPs. The image shows that the NPs are well-dispersed, and the size of the NPs size appears to be consistent with the size calculated using the Debye–Scherrer formula in the XRD analysis. Spherical-shaped NPs with a particle size smaller than 5 nm were formed, which is confirmed via the TEM images shown in Figure 4 and is consistent with the FESEM results. The crystal lattice fringe spacings of 0.329 nm are for the (110) plane, as shown in Figure 4A [28]. Furthermore, the highly crystalline structure of SnO2 is indicated through the selected area electron diffraction (SAED), as shown in Figure 4B. The diffraction circles from small to large represent (110), (101), and (211) planes of rutile-structured SnO2, respectively, in agreement with the XRD data. This clearly indicates that the synthesized N:SnO2 NPs are highly crystalline and possess a well-defined structure.
The highly crystalline nature of the synthesized N:SnO2 NPs is of great importance for their photocatalytic application [29,30,31]. This allows for efficient charge transfer to occur, resulting in an enhancement of the photocatalytic activity of the NPs. The observed crystal lattice fringe spacings and the SAED pattern confirm the good quality of the synthesized N:SnO2 NPs and suggest their potential use as highly efficient photocatalysts.

3.3. TGA Analysis

TGA analysis is a frequently employed method used to study the thermal endurance of substances. In the case of N:SnO2 NP photocatalysts, the TGA curve demonstrated in Figure 5 illustrates the weight loss of the sample as a function of temperature. The curve shows two weight loss regions, one below 200 °C and the other between 200 °C to 800 °C. Firstly, an evident 7% weight loss was observed at temperatures below 200 °C [32]. This weight change observed in the photocatalyst was caused by the removal of adsorbed water and gases from its surface. Additionally, a 7% weight loss was observed within the temperature range of 200 °C to 800 °C, indicating that other substances in the photocatalyst were being eliminated. This could be due to the decomposition of organic compounds or other volatile species that may have been present in the sample. The rate of weight loss in this region was slower than the first region, indicating that the decomposition process was slower. However, no significant change in weight was noticed above 800 °C, suggesting that the photocatalyst remained stable at high temperatures due to its inorganic composition of SnO2. Therefore, it is recommended to set the calcination temperature for N:SnO2 NPs to 800 °C to maintain the catalyst’s stability. It is important to note that more details about the experiment are required to fully understand the context of these observations. For example, the heating rate, sample mass, and atmosphere during the TGA analysis can all influence the results. Nevertheless, the TGA curve offers significant insights into the N:SnO2 photocatalyst’s thermal stability and can be used to optimize the calcination temperature for the synthesis of the material.

3.4. Surface Area Analysis

The N2 adsorption/desorption isotherm of the N:SnO2 NPs at 77 K has been presented in our previous published paper. The Barrett–Joyner–Halenda (BJH) method revealed the pore volume, pore size, and specific surface area to be 13.59 cc/g, 3.82 nm, and 139.7 m2/g, respectively. At relative pressures between 0.3–1.0, the adsorption/desorption graph (Figure 6) displays a type IV isotherm with an H3 hysteresis loop, which is evidence of mesoporosity [19].

3.5. Photocatalytic Activity of Carcinogenic Dyes

Photocatalytic dye degradation of MB, MO, and CV in aqueous solution was carried out using N:SnO2 NPs under UV light irradiation. Nevertheless, the degradation efficiency of these dyes using N:SnO2 NPs was also investigated in the presence of EDTA as sacrificial agent when exposed to UV light irradiation. The pure SnO2 NPs do not exhibit any photodegradation ability for any of the mentioned aqueous dye solution. The results demonstrated less than 10% degradation of the reported dyes in the aqueous solutions, even after 90 min of irradiation under UV light. The incorporation of N to the surface of SnO2 greatly improved the activity of the desired N:SnO2 NPs. Figure 7 illustrates the UV-Vis absorption of the reported dyes over time during exposure to UV light. It can be observed distinctly that the absorbance decreased exceptionally after irradiation within a maximum of 90 min for the N:SnO2 NP photocatalyst. Figure S1 illustrates the photocatalytic degradation of the MB dye as a function of the irradiation time for the N:SnO2 NPs. In Figure S2 the bottle numbered with ‘0’ contains the standard solution, and the one numbered with ‘1’ contains the solution after 30 min. Stirring of the dye with the sample was conducted in the dark, and further samples were collected at intervals of 15 min. The analysis showed that the performance of the N:SnO2 NPs improves up to 50 min, and then declines as the photo-reduction time increases up to 70 min. The photodegradation efficiency of MB could reach up to 93% during an irradiation time of 75 min. Similarly, Figure S3 depicts the photodegradation of the MO dye. It is observed that the performance of the N:SnO2 NPs increases during up to 90 min of photo-reduction time. The degradation efficiency of MO could reach up to 84% over 90 min. Likewise, Figures S4 and S5 uncloaked the photodegradation of the CV dye. It can be elucidated that the photocatalytic ability of the N:SnO2 NPs increases during the first 30 min and then decreases until 75 min of photo-reduction time has elapsed. The degradation efficiency of CV could reach up to 73% in 90 min. However, the pure SnO2 NPs were only capable of decomposing small quantities of the respective dyes. Notably, the photocatalytic test was repeated more than twice under the same experimental set-up to assess the photodegradation ability of the N:SnO2 NPs. Thus, the derived results evinced that N:SnO2 NPs exhibited improved photocatalysis in the degradation of carcinogenic dye solutions.
The photocatalytic degradation of various dyes was also performed using synthesized NPs along with EDTA as a sacrificial reagent (Figure 7). The results show that with EDTA, N:SnO2 degraded ~90% of the MB dye, 88% of the CV dye, and 86% of the MO dye within 15 min of UV light irradiation. This enhanced degradation performance owes to the hole, superoxide ( O 2 ) radical, and hydroxyl (•OH) radical. EDTA restricted the recombination of electron–hole pairs by capturing the holes [33], and hence resulted in better degradation as compared to those where no EDTA was used.
After successful catalysis, the stability of the used N:SnO2 NPs was further assessed. To do so, the PXRD pattern of the after-reaction photocatalyst was plotted as shown in Figure S6. As clearly illustrated, the observed crystallographic peaks correspond exactly with the SnO2 tetragonal phase. Furthermore, no diminished, weakened, or unwanted reflections of diffraction peaks were identified, thus indicating the durability and integrity of the N:SnO2 NPs.

3.6. Photocatalytic Mechanism of Dye Degradation

To comprehend the likely mechanism of photocatalysis of carcinogenic dyes such as MB, MO, and CV by N:SnO2 NPs and determine a definitive insight on the same, the band gap position of the synthesized N:SnO2 NPs catalyst must be unraveled. This is due to the aspects of photo-excited electrons and holes mediating excitation, transport, and recombination. In the previous study conducted by Bhawna et al., the band gap assessment was conducted and the conduction band (CB) and the valence band (VB) edge positions of the N:SnO2 NPs was theoretically computed to be −1.13 eV and 2.32 eV, respectively [19]. The band gap of SnO2 in its pure form is 3.6 eV, as reported in the literature [2]. However, when doped with N, N:SnO2 now possesses a modified band gap of 3.45 eV, as calculated in our previous research using a UV-Visible spectrum [5,19]. This shift in band gap has been explained as a result of an N substitution in the SnO2 crystal structure and the overlap of O (2p) and N (2p) orbitals. The FTIR data from our previous research article state that doping substitutes the O atom into a tin lattice with an N atom, resulting in lattice oxygen vacancies which are responsible for the photocatalytic performance of N:SnO2 NPs [19]. The possible mechanism of photocatalysis of N:SnO2 NPs was schematically represented in Figure 8.
Figure 8 illustrates the likely mechanism for the breakdown of MB, MO, and CV dyes using N:SnO2 NPs. When the photocatalyst is exposed to light irradiation, electrons in the VB were stimulated into the CB. These electrons move to the catalyst’s surface to contribute to surface reactions. Oxygen molecules adsorbed or dissolved in water react with the electrons at the surface, leading to the formation of O 2 . Additionally, •OH is created when holes in the VB interact with water molecules or OH ions.
The O 2 and •OH are highly reactive oxidizing agents that can react with organic dyes. These agents attack the dye molecules, leading to their oxidative breakdown and the production of less toxic compounds. The degradation efficiency of N:SnO2 NPs has been attributed to the lattice disorder and charge imbalance created in the tin lattice on incorporation of N ions. The presence of N ions enhances the separation of photo-excited electron–hole pairs and increases the number of active sites for photocatalysis, resulting in the improved photocatalytic activity of the N:SnO2 NPs.
Overall, the mechanism shown in Figure 8 provides insights into the working principle behind the degradation of organic dyes utilizing N:SnO2 NPs and highlights the importance of charge separation and active sites for efficient photocatalytic activity.

4. Conclusions

In this report, we have successfully synthesized N:SnO2 NPs using a one-step facile synthetic strategy and investigated their potential as a photocatalyst for carcinogenic dye degradation. The structural and morphological studies of N:SnO2 NPs were confirmed, demonstrating their uniform size distribution and crystalline nature, through several characterization tools such as PXRD, FESEM, TGA, and others. The synthesized N:SnO2 NPs have been explored as excellent photocatalysts that could efficiently degrade up to 93% of the MB dye, 83% of the MO dye, and 73% of the CV dye under UV light irradiation. Additionally, the role of EDTA as a sacrificial agent was also investigated for these dyes. It can be elucidated that ~90% of these dyes degraded within 15 min when exposed to UV light and exhibited the potent efficiency of the synthesized NPs.
Future studies could investigate the underlying mechanism and role of sacrificial agents responsible for the high photocatalytic efficiency for degradation of N:SnO2 NPs. The efficiency and simplicity of the one-step synthesis method for N:SnO2 NPs make them an attractive candidate for use in various industries and research fields. Therefore, the findings of this study could have a considerable influence on the advancement of sustainable and eco-friendly technologies for wastewater treatment and pollution control.

Supplementary Materials

The following supporting information can be downloaded at: https://www.mdpi.com/article/10.3390/separations10060322/s1, Figure S1: temporal absorption spectrum changes of methylene blue (MB) aqueous solution in the presence of N:SnO2 NPs under UV light irradiation; Figure S2: color disappearance of MB aqueous solution in the presence of N:SnO2 NPs under UV light irradiation; Figure S3: the temporal absorption spectrum changes of methyl orange (MO) aqueous solution in the presence of N:SnO2 NPs under UV light irradiation; Figure S4: the temporal absorption spectrum changes of crystal violet (CV) aqueous solution in the presence of N:SnO2 NPs under UV light irradiation; Figure S5: color disappearance of CV aqueous solution in the presence of N:SnO2 NPs under UV light irradiation; Figure S6: comparative PXRD pattern of N:SnO2 nanoparticles: before (black) and after (red) catalysis; Table S1: calculation of parameters of N:SnO2 nanoparticles.

Author Contributions

Conceptualization, V.K. (Vinod Kumar); methodology, B. and V.K. (Vinod Kumar) software, B., S.K. and R.S.; validation, V.K. (Vandana Kumari), R.K. and A.K.M.; formal analysis, B. and V.K. (Vinod Kumar); investigation, B. and S.K.; resources, B., S.K. and R.S.; data curation, B.; writing—original draft preparation, B., S.K., R.S. and V.K. (Vinod Kumar); writing—review and editing, R.K., P.K.S., V.K. (Vandana Kumari) and A.K.M.; visualization, R.K., P.K.S., V.K. (Vandana Kumari) and A.K.M.; supervision, V.K. (Vinod Kumar) All authors have read and agreed to the published version of the manuscript.

Funding

This research received no external funding.

Data Availability Statement

Data will be available on request.

Acknowledgments

Authors Bhawna and Sanjeev Kumar thank UGC and CSIR (08/694(0004)/2018-EMR-I) for Senior Research Fellowship, respectively. The authors also thank USIC, Department of Chemistry, University of Delhi and SCNS, JNU for various characterizations.

Conflicts of Interest

The authors declare that they have no known competing and financial interest that could have appeared to influence the work reported in this paper.

References

  1. Raza, A.; Altaf, S.; Ali, S.; Ikram, M.; Li, G. Recent advances in carbonaceous sustainable nanomaterials for wastewater treatments. Sustain. Mater. Technol. 2022, 32, e00406. [Google Scholar] [CrossRef]
  2. Bhawna; Kumar, S.; Sharma, R.; Gupta, A.; Tyagi, A.; Singh, P.; Kumar, A.; Kumar, V. Recent insights into SnO2-based engineered nanoparticles for sustainable H2 generation and remediation of pesticides. New J. Chem. 2022, 46, 4014–4048. [Google Scholar] [CrossRef]
  3. Ambigadevi, J.; Kumar, P.S.; Vo, D.-V.N.; Haran, S.H.; Raghavan, T.S. Recent developments in photocatalytic remediation of textile effluent using semiconductor based nanostructured catalyst: A review. J. Environ. Chem. Eng. 2021, 9, 104881. [Google Scholar] [CrossRef]
  4. Islam, M.A.; Ali, I.; Karim, S.A.; Firoz, M.S.H.; Chowdhury, A.-N.; Morton, D.W.; Angove, M.J. Removal of dye from polluted water using novel nano manganese oxide-based materials. J. Water Process Eng. 2019, 32, 100911. [Google Scholar] [CrossRef]
  5. Sun, C.; Yang, J.; Xu, M.; Cui, Y.; Ren, W.; Zhang, J.; Zhao, H.; Liang, B. Recent intensification strategies of SnO2-based photocatalysts: A review. Chem. Eng. J. 2022, 427, 131564. [Google Scholar] [CrossRef]
  6. Robinson, T.; McMullan, G.; Marchant, R.; Nigam, P. Remediation of dyes in textile effluent: A critical review on current treatment technologies with a proposed alternative. Bioresour. Technol. 2001, 77, 247–255. [Google Scholar] [CrossRef]
  7. Raza, A.; Zhang, Y.; Cassinese, A.; Li, G. Engineered 2D Metal Oxides for Photocatalysis as Environmental Remediation: A Theoretical Perspective. Catalysts 2022, 12, 1613. [Google Scholar] [CrossRef]
  8. Islam, M.A.; Morton, D.W.; Johnson, B.B.; Mainali, B.; Angove, M.J. Manganese oxides and their application to metal ion and contaminant removal from wastewater. J. Water Process Eng. 2018, 26, 264–280. [Google Scholar] [CrossRef]
  9. Islam, M.A.; Morton, D.W.; Johnson, B.B.; Pramanik, B.K.; Mainali, B.; Angove, M.J. Metal ion and contaminant sorption onto aluminium oxide-based materials: A review and future research. J. Environ. Chem. Eng. 2018, 6, 6853–6869. [Google Scholar] [CrossRef]
  10. Dheyab, M.A.; Aziz, A.A.; Jameel, M.S.; Oladzadabbasabadi, N. Recent advances in synthesis, modification, and potential application of tin oxide nanoparticles. Surf. Interfaces 2022, 28, 101677. [Google Scholar] [CrossRef]
  11. Rajput, R.B.; Kale, R.B. Hydro/solvothermally synthesized visible light driven modified SnO2 heterostructure as a photocatalyst for water remediation: A review. Environ. Adv. 2021, 5, 100081. [Google Scholar] [CrossRef]
  12. Hong, X.; Wang, X.; Li, Y.; Fu, J.; Liang, B. Progress in graphene/metal oxide composite photocatalysts for degradation of organic pollutants. Catalysts 2020, 10, 921. [Google Scholar] [CrossRef]
  13. Hassan, J.Z.; Raza, A.; Qumar, U.; Li, G. Recent advances in engineering strategies of Bi-based photocatalysts for environmental remediation. Sustain. Mater. Technol. 2022, 33, e00478. [Google Scholar] [CrossRef]
  14. Saeed, M.; Muneer, M.; Haq, A.u.; Akram, N. Photocatalysis: An effective tool for photodegradation of dyes—A review. Environ. Sci. Pollut. Res. 2022, 29, 293–311. [Google Scholar] [CrossRef]
  15. Xu, L.; Steinmiller, E.M.; Skrabalak, S.E. Achieving synergy with a potential photocatalytic Z-scheme: Synthesis and evaluation of nitrogen-doped TiO2/SnO2 composites. J. Phys. Chem. C 2012, 116, 871–877. [Google Scholar] [CrossRef]
  16. Sharma, S.; Kumar, N.; Makgwane, P.R.; Chauhan, N.S.; Kumari, K.; Rani, M.; Maken, S. TiO2/SnO2 nano-composite: New insights in synthetic, structural, optical and photocatalytic aspects. Inorg. Chim. Acta 2022, 529, 120640. [Google Scholar] [CrossRef]
  17. Chen, Y.; Jiang, Y.; Chen, B.; Ye, F.; Duan, H.; Cui, H. Facile fabrication of N-doped carbon quantum dots modified SnO2 composites for improved visible light photocatalytic activity. Vacuum 2021, 191, 110371. [Google Scholar] [CrossRef]
  18. Liu, S.-Y.; Wang, Q.; Ou, L.-H.; Du, H.-L.; Long, Y.; Zhen, W.-J. Solid-Phase Synthesis of Non-metal (S, N)-Doped Tin Oxide Nanopowders at Room Temperature and its Photodegradation Properties for Wastewater of Biomass Treatment. J. Inorg. Organomet. Polym. Mater. 2022, 32, 2748–2762. [Google Scholar] [CrossRef]
  19. Bhawna; Gupta, A.; Kumar, P.; Tyagi, A.; Kumar, R.; Kumar, A.; Singh, P.; Singh, R.; Kumar, V. Facile Synthesis of N-Doped SnO2 Nanoparticles: A Cocatalyst-Free Promising Photocatalyst for Hydrogen Generation. ChemistrySelect 2020, 5, 7775–7782. [Google Scholar] [CrossRef]
  20. Kumar, V.; Choudhary, A.K.; Kumar, P.; Sharma, S. Nanotechnology: Nanomedicine, nanotoxicity and future challenges. Nanosci. Nanotechnol.-Asia 2019, 9, 64–78. [Google Scholar] [CrossRef]
  21. Bail, L.; Armel; Duroy, H.; Fourquet, J.L. Ab-initio structure determination of LiSbWO6 by X-ray powder diffraction. Mater Res. Bull 1988, 23, 447–452. [Google Scholar] [CrossRef]
  22. Rodríguez-Carvajal, J. Recent advances in magnetic structure determination by neutron powder diffraction. Phys. B Condens. Matter 1993, 192, 55–69. [Google Scholar] [CrossRef]
  23. Shannon, R.D. Revised effective ionic radii and systematic studies of interatomic distances in halides and chalcogenides. Acta crystallogr. A 1976, 32, 751–767. [Google Scholar] [CrossRef]
  24. Kumar, S.; Yadav, S.K.; Gupta, A.; Kumar, R.; Ahmed, J.; Chaudhary, M.; Kumar, V. B-doped SnO2 nanoparticles: A new insight into the photocatalytic hydrogen generation by water splitting and degradation of dyes. Environ. Sci. Pollut. Res. 2022, 29, 47448–47461. [Google Scholar] [CrossRef]
  25. Kumar, V.; Bhawna; Yadav, S.K.; Gupta, A.; Dwivedi, B.; Kumar, A.; Singh, P.; Deori, K. Facile synthesis of Ce–doped SnO2 nanoparticles: A promising photocatalyst for hydrogen evolution and dyes degradation. ChemistrySelect 2019, 4, 3722–3729. [Google Scholar] [CrossRef]
  26. Kumar, V.; Uma, S.; Nagarajan, R. Optical and magnetic properties of (Er, F) co-doped SnO2 nanocrystals. Turk. J. Phys. 2014, 38, 450–462. [Google Scholar] [CrossRef]
  27. Williamson, G.; Hall, W. X-ray line broadening from filed aluminium and wolfram. Acta Metall. 1953, 1, 22–31. [Google Scholar] [CrossRef]
  28. Sun, P.; Zhou, X.; Wang, C.; Wang, B.; Xu, X.; Lu, G. One-step synthesis and gas sensing properties of hierarchical Cd-doped SnO2 nanostructures. Sens. Actuators B Chem. 2014, 190, 32–39. [Google Scholar] [CrossRef]
  29. Luque, P.A.; Nava, O.; Soto-Robles, C.A.; Chinchillas-Chinchillas, M.J.; Garrafa-Galvez, H.E.; Baez-Lopez, Y.A.; Valdez-Núñez, K.P.; Vilchis-Nestor, A.R.; Castro-Beltrán, A. Improved photocatalytic efficiency of SnO2 nanoparticles through green synthesis. Optik 2020, 206, 164299. [Google Scholar] [CrossRef]
  30. Pan, H. Principles on design and fabrication of nanomaterials as photocatalysts for water-splitting. Renew. Sust. Energ. Rev. 2016, 57, 584–601. [Google Scholar] [CrossRef]
  31. Huang, D.; Li, Z.; Zeng, G.; Zhou, C.; Xue, W.; Gong, X.; Yan, X.; Chen, S.; Wang, W.; Cheng, M. Megamerger in photocatalytic field: 2D g-C3N4 nanosheets serve as support of 0D nanomaterials for improving photocatalytic performance. Appl. Catal. B Environ. 2019, 240, 153–173. [Google Scholar] [CrossRef]
  32. Aslam, M.; Mahmood, T.; Naeem, A.; Ali, R. Investigation of HDTMA mediated sol gel synthesis of N-doped SnO2 nanoparticles: Studies of their electrical and optical properties. Mater. Technol. 2021, 36, 169–178. [Google Scholar] [CrossRef]
  33. Jin, K.; Mian, M.; Li, X.; Wang, R.; Zhao, Y.; Li, Y.; Wang, H. A low-dosage silver-loaded flower-like Bi2WO6 nanosheets toward efficiently photocatalytic degradation of sulfamethoxazole. Mater. Sci. Semicond. Process. 2022, 139, 106338. [Google Scholar] [CrossRef]
Figure 1. The PXRD pattern of the N:SnO2 nanoparticles.
Figure 1. The PXRD pattern of the N:SnO2 nanoparticles.
Separations 10 00322 g001
Figure 2. The W–H plot of the N:SnO2 nanoparticles.
Figure 2. The W–H plot of the N:SnO2 nanoparticles.
Separations 10 00322 g002
Figure 3. (A) FESEM micrograph, (B) EDAX, and (C) elemental mapping of N:SnO2 nanoparticles.
Figure 3. (A) FESEM micrograph, (B) EDAX, and (C) elemental mapping of N:SnO2 nanoparticles.
Separations 10 00322 g003
Figure 4. TEM image of (A) crystal lattice fringe, and (B) SAED pattern of N:SnO2 nanoparticles.
Figure 4. TEM image of (A) crystal lattice fringe, and (B) SAED pattern of N:SnO2 nanoparticles.
Separations 10 00322 g004
Figure 5. TGA curve of N:SnO2 nanoparticles.
Figure 5. TGA curve of N:SnO2 nanoparticles.
Separations 10 00322 g005
Figure 6. Barrett–Joyner–Halenda graph of N:SnO2 nanoparticles.
Figure 6. Barrett–Joyner–Halenda graph of N:SnO2 nanoparticles.
Separations 10 00322 g006
Figure 7. Photocatalytic degradation of Methylene Blue (MB), Methyl Orange (MO), and Crystal Violet (CV) dyes independently and along with EDTA as a sacrificial agent.
Figure 7. Photocatalytic degradation of Methylene Blue (MB), Methyl Orange (MO), and Crystal Violet (CV) dyes independently and along with EDTA as a sacrificial agent.
Separations 10 00322 g007
Figure 8. Illustration demonstrating the photocatalytic mechanism of N:SnO2 nanoparticles.
Figure 8. Illustration demonstrating the photocatalytic mechanism of N:SnO2 nanoparticles.
Separations 10 00322 g008
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content.

Share and Cite

MDPI and ACS Style

Bhawna; Sharma, R.; Kumar, S.; Kumar, R.; Sahu, P.K.; Kumari, V.; Mishra, A.K.; Kumar, V. Unlocking the Potential of N-Doped SnO2 for Sustainable Photocatalytic Degradation of Carcinogenic Dyes. Separations 2023, 10, 322. https://doi.org/10.3390/separations10060322

AMA Style

Bhawna, Sharma R, Kumar S, Kumar R, Sahu PK, Kumari V, Mishra AK, Kumar V. Unlocking the Potential of N-Doped SnO2 for Sustainable Photocatalytic Degradation of Carcinogenic Dyes. Separations. 2023; 10(6):322. https://doi.org/10.3390/separations10060322

Chicago/Turabian Style

Bhawna, Ritika Sharma, Sanjeev Kumar, Ravinder Kumar, Prasanta Kumar Sahu, Vandana Kumari, Ajay Kumar Mishra, and Vinod Kumar. 2023. "Unlocking the Potential of N-Doped SnO2 for Sustainable Photocatalytic Degradation of Carcinogenic Dyes" Separations 10, no. 6: 322. https://doi.org/10.3390/separations10060322

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.

Article Metrics

Back to TopTop