Next Article in Journal
From Prediction to Prevention: Leveraging Deep Learning in Traffic Accident Prediction Systems
Previous Article in Journal
A Blockchain-Based Framework for Rural Property Rights Transactions
 
 
Font Type:
Arial Georgia Verdana
Font Size:
Aa Aa Aa
Line Spacing:
Column Width:
Background:
Communication

Investigation of the Effect of Different SiNx Thicknesses on the Characteristics of AlGaN/GaN High-Electron-Mobility Transistors in Ka-Band

1
Department of Materials Science and Engineering, National Yang Ming Chiao Tung University, Hsinchu City 30010, Taiwan
2
International College of Semiconductor Technology, National Yang Ming Chiao Tung University, Hsinchu City 30010, Taiwan
*
Author to whom correspondence should be addressed.
Electronics 2023, 12(20), 4336; https://doi.org/10.3390/electronics12204336
Submission received: 3 October 2023 / Revised: 15 October 2023 / Accepted: 17 October 2023 / Published: 19 October 2023
(This article belongs to the Special Issue Challenges, Innovation and Future Perspectives of GaN Technology)

Abstract

:
The effect of different SiNx thicknesses on the performance of AlGaN/GaN high-electron-mobility transistors (HEMTs) was investigated in this paper. The current, transconductance (Gm), cut-off frequency (fT), maximum oscillation frequency (fmax), power performance, and output third-order intercept point (OIP3) of devices with three different SiNx thicknesses (150 nm, 200 nm, and 250 nm) were measured and analyzed. The DC measurements revealed an increase in both the drain-source current (IDS) and Gm values of the device with increasing SiNx thickness. The S-parameter measurement results show that devices with a higher SiNx thickness exhibit improved fT and fmax. Regarding power performance, thicker SiNx devices also improve the output power density (Pout) and power-added efficiency (PAE) in the Ka-band. In addition, the two-tone measurement results at 28 GHz show that the OIP3 increased from 35.60 dBm to 40.87 dBm as the SiNx thickness increased from 150 nm to 250 nm. The device’s characteristics improved by appropriately increasing the SiNx thickness.

1. Introduction

Recently, extensive research has been conducted on the application of AlGaN/GaN high-electron-mobility transistors (HEMTs) in high-frequency microwave power devices, ranging from essential everyday needs to defense applications such as 5G small-cell base stations, satellite communications, defense and military applications, and industrial radar [1,2,3,4,5,6]. Compared to other III-V compound semiconductors, GaN materials possess excellent characteristics, such as a wide bandgap, high electron mobility, high saturation velocity, and a high breakdown field [7,8,9]. Additionally, the combination of GaN and AlGaN layers forms a two-dimensional electron gas (2DEG) at the interface, which is characterized by a high electron concentration. These excellent characteristics allow GaN devices to maintain high output power at higher frequencies [10,11,12].
In the face of the arrival and commercialization of the fifth generation of mobile communication (5G), characterized by faster transmission speeds, low latency, large bandwidth, and high density, it is advantageous for the development of services such as big data, the Internet of Things (IoT), and Artificial Intelligence (AI) [13,14]. These advancements can drive high-quality audiovisual entertainment, self-driving cars, drones, smart healthcare, intelligent factories, smart retail, smart cities, and other value-added innovative applications. This has become a focal point of development in countries around the world. Due to the growing demand for high-speed transmission in 5G communication, there is an increasing need for high-frequency devices operating in the Ka-band to support wider bandwidth requirements [15,16,17,18].
In wireless communication, when two or more signals pass through nonlinear amplifier devices, intermodulation distortion (IMD) occurs. Because IMD generates unwanted spurious emissions, it leads to an increase in the occupied bandwidth and interferes with adjacent channels, ultimately reducing audio clarity or increasing spectral occupancy. Among the nonlinear distortions generated by devices within the system, the third-order intermodulation distortion (IM3) is the most influential factor [19,20,21]. It is closest to the main signal, difficult to filter out, and easily affects the signal quality. Therefore, improving device linearity by enhancing the performance metrics, including the output third-order intercept point (OIP3) and reducing IM3, is an important concern. The literature has put forward various methods to enhance HEMT linearity, including δ-Doped [22], gate dielectric [23], N-Polar GaN MIS-HEMT [24], selective-area charge implantation [25], fin-like configuration [26], and etched-fin gate structure [27]. For traditional AlGaN/GaN HEMTs, the transconductance (Gm) of the device rapidly decreases after reaching its peak as the gate-source voltage (VGS) increases, resulting in severe nonlinearity [28]. To improve the DC characteristics of a device, many studies have proposed methods such as modifying the device structure or reducing the gate leakage current to enhance the overall DC and RF performance of the device [29,30,31,32]. However, there is limited literature on improving device performance by increasing the SiNx thickness [33].
In this study, we investigate the effect of different SiNx thicknesses on the characteristics of AlGaN/GaN HEMT devices in the Ka-band. The DC characteristics, S-parameter measurement, power performance, and OIP3 of devices with three different SiNx thicknesses (150 nm, 200 nm, and 250 nm) were measured. The measurement results demonstrate an enhancement in the device’s performance as the SiNx thickness increases to 250 nm.

2. Materials and Methods

The AlGaN/GaN HEMT heterostructure used in this study was grown on a 4-inch SiC substrate using metal–organic chemical vapor deposition (MOCVD). A cross-sectional schematic diagram of the AlGaN/GaN HEMT is displayed in Figure 1. The dimensions of the device were as follows: Lg is 150 nm, Hhead is 350 nm, and the thicknesses of the SiNx layer (tSiNx) were 150 nm, 200 nm, or 250 nm. The device fabrication process flow is shown in Figure 2. Device fabrication began with the Ohmic contact formation of Ti/Al/Ni/Au. The Ohmic metal layers were deposited using an E-gun evaporator, followed by rapid thermal annealing (RTA) at 830 °C for 30 s in a nitrogen atmosphere to form Ohmic contacts. Next, device isolation was achieved using boron ion implantation. A photoresist was used as a mask to protect the active region, and boron ions (B11+) were implanted using an ion implantation machine to complete the device isolation process. To define the gate region, the first SiNx passivation layer was deposited using plasma-enhanced chemical vapor deposition (PECVD). The thicknesses of the first SiNx layers (tSiNx) were 150 nm, 200 nm, and 250 nm. Afterward, stepper lithography was performed twice to complete the gate fabrication. The first step of stepper lithography defined the areas for etching the first SiNx film, followed by etching using inductively coupled plasma (ICP). The second step of stepper lithography defined the areas for depositing the gate metal. After two steps of stepper lithography, the Ni/Au gate metal stack was deposited using an E-gun evaporator to complete the gate fabrication. Before depositing the gate metal, the wafer was immersed in a diluted HCl solution for one minute to remove any natural oxides from the AlGaN barrier layer. After gate fabrication was completed, the first SiNx layer was removed using ICP, followed by the deposition of the second SiNx layer using PECVD. Finally, for metallization, holes were opened in the passivation film via ICP, and then a 1.5 µm thickness of Au metallization layer was deposited.

3. Results and Discussion

The DC characteristics of the 4 × 50 μm AlGaN/GaN HEMTs were measured using Keysight B1505A. Figure 3 shows the typical IDS-VGS and Gm-VGS characteristics at VDS = 20 V for 4 × 50 μm AlGaN/GaN HEMT devices with different SiNx thicknesses (150 nm, 200 nm, and 250 nm). While the SiNx thickness increases from 150 nm to 200 nm, the device exhibits an increase in the saturation drain current (IDSS) from 766.5 mA/mm to 861 mA/mm, and the maximum transconductance (Gm,max) increases from 290.1 mS/mm to 312.9 mS/mm. Increasing the SiNx thickness to 250 nm no longer significantly increases the IDSS and Gm,max of the device, as shown in Table 1. Compared to other thicknesses, the device with a SiNx thickness of 250 nm exhibits the highest IDSS and Gm,max. The increase in the device’s current and Gm is due to the increase in the thickness of the SiNx passivation layer, which leads to an increase in the biaxial tensile stress applied to the AlGaN layer, further increasing the surface charge density at the heterointerface [34,35]. Furthermore, the threshold voltage (Vth) for a 150 nm SiNx thickness is −3.1 V, whereas the Vth for SiNx thicknesses of both 200 nm and 250 nm is −3.7 V. The Vth is defined as the VGS when IDS = 1 mA/mm.
To further analyze the linearity, a polynomial curve fitting technique is applied to the transfer characteristic function of these devices, as shown in Equation (1) [36].
I D S V G S = a 0 + a 1 V G S + a 2 V G S 2 + a 3 V G S 3 + a 4 V G S 4 + a 5 V G S 5
In addition, Equation (2) can be used to estimate the IM3 levels generated by the device [37]. Equation (3) illustrates the relationship between OIP3, transconductance (Gm), drain conductance (Gds), and Gm″ [38].
IM 3 = 3 8 a 3 A 3 + 50 32 a 5 A 5
OIP 3   ( G m ) 3 G m G d s 2 R L
The linearity of the device is primarily determined by the flatness of the Gm profile. In other words, the coefficient a 1 should be larger, whereas the ratios a 3 / a 1 and a 5 / a 1 should be minimized [39]. The polynomial curve fitting coefficients and the gate voltage swing (GVS), defined as a 10% drop in Gm,max, are presented in Table 1. Compared to devices with SiNx thicknesses of 150 nm and 200 nm, the device with a SiNx thickness of 250 nm exhibits lower a 3 / a 1 and a 5 / a 1 values, indicating that the device with a SiNx thickness of 250 nm has better linearity. Furthermore, the two-tone measurement results at the end of the article also indicate an improvement in the linearity of the devices with thicker SiNx.
Next, the S-parameters of the 4 × 50 μm devices with different SiNx thicknesses (150, 200, and 250 nm) were measured using a Keysight E8361A PNA Network Analyzer in the frequency range from 100 MHz to 67 GHz, as shown in Figure 4. The values of fT can be obtained by converting the measured S-parameters to H-parameters, whereas the values of fmax can be obtained by extrapolating the gain curve with a slope of −20 dB/decade. When increasing the SiNx thickness from 150 nm to 250 nm, the fT value increases from 33.7 GHz to 53.1 GHz, as indicated in Table 2. Furthermore, there is an increase in fmax, which improves from 76.9 GHz to 138.9 GHz. The gate stem height changes due to the varying SiNx thicknesses. According to the definitions of fT and fmax in Equations (4) and (5), increasing the SiNx thickness to enhance the device’s Gm will result in higher fT and fmax values [40]. Increasing the gate stem height also reduces Cgs and Cgd, further enhancing the fT and fmax of the device [40]. Moreover, Cgs will also be affected when the gate is facing towards the drain side [41]. However, increasing the gate stem height to 300 nm does not lead to a further significant reduction in the capacitance [42]. Additionally, higher gate stem heights contribute to an increase in the gate resistance (Rg) of the device.
f T = g m / 2 π C g s + C g d × [ 1 + ( R s + R d ) g 0 ] + g m C g d ( R s + R d ) g m 2 π C g s + C g d
f m a x = f T 2 g 0 ( R g + R s ) + 2 f T C g d R g
Figure 5 shows the load-pull measurement results at 28 GHz for 4 × 50 μm devices with three different SiNx thicknesses (150 nm, 200 nm, and 250 nm). All devices were measured at a bias of class AB (1/4 IDSS, IDSS = IDS at VGS = 0) and VDS = 20 V. When increasing the SiNx thickness of the device from 150 nm to 200 nm, the maximum output power density (Pout,max) increases from 2.21 W/mm to 2.61 W/mm. Furthermore, when increasing the SiNx thickness from 200 nm to 250 nm, Pout,max increases from 2.61 W/mm to 2.72 W/mm. From the load-pull measurement results, it can be observed that the Pout, PAE, and linear gain of the device show improvement when the SiNx thickness is increased from 150 nm to 250 nm. The device with a 250 nm SiNx thickness exhibits the best power performance, with a Pout,max of 2.72 W/mm, PAEmax of 31.78%, and a linear gain of 10.68 dB. Therefore, increasing the thickness of SiNx improves the power performance of the device.
To evaluate the linearity of the devices, two-tone measurements were performed at 28 GHz with a 5 MHz tone spacing using the Keysight E8267D signal generator, N9030B spectrum analyzer, U84888A power sensor, N6700C modular power system, and an AMP4072 power amplifier. Figure 6 shows the two-tone measurement results at 28 GHz for 4 × 50 μm devices with different SiNx thicknesses. During the measurements, each device was measured at a bias of class AB (1/4 IDSS, IDSS = IDS at VGS = 0) and VDS = 20 V. The measurement results show that the OIP3 value improves from 35.60 dBm to 40.87 dBm when the SiNx thickness of the device is increased from 150 nm to 250 nm. Based on the previous polynomial curve fitting results, it can be observed that as the SiNx thickness increases, the ratios of a 3 / a 1 and a 5 / a 1 decrease, resulting in an improvement in the device’s linearity. Moreover, the increase in OIP3 could be attributed to the increase in SiNx thickness, which leads to a higher current and changes in the Gm distribution, thereby enhancing the linearity of the device.

4. Conclusions

In this paper, the effects of increasing the SiNx thickness on the characteristics of AlGaN/GaN HEMTs were investigated. The DC measurement results indicate that as the SiNx thickness increases, the current and Gm for the device also increase. The device’s fT and fmax also improve with an increase in the SiNx thickness. For the 4 × 50 μm device with a SiNx thickness of 250 nm, the load-pull measurement results at 28 GHz show a Pout,max of 2.72 W/mm, a PAEmax of 31.78%, and a linear gain of 10.68 dB. Furthermore, the two-tone measurement results show that the improvement in OIP3 is due to the increase in the current for the device, resulting in a change in the Gm profile. The final results show that when the SiNx thickness of the device increases from 150 nm to 200 nm, and even up to 250 nm, its characteristics such as IDSS, Gm,max, Pout,max, fT, fmax, and OIP3 improve. Thus, we have demonstrated that device characteristics can be improved by increasing the SiNx thickness to a sufficient value, such as 250 nm.

Author Contributions

Conceptualization, C.-W.H. and Y.-C.L.; methodology, C.-W.H. and Y.-C.L.; validation, Y.-C.L.; investigation, C.-W.H.; resources, E.-Y.C.; data curation, C.-W.H. and Y.-C.L.; writing—original draft preparation, C.-W.H.; writing—review and editing, C.-W.H., Y.-C.L., M.-W.L., and E.-Y.C.; supervision, Y.-C.L. and E.-Y.C.; project administration, Y.-C.L. and E.-Y.C.; funding acquisition, E.-Y.C. All authors have read and agreed to the published version of the manuscript.

Funding

This study was financially supported by the “Center for the Semiconductor Technology Research” from The Featured Areas Research Center Program within the framework of the Higher Education Sprout Project by the Ministry of Education (MOE) in Taiwan. This study was also supported in part by the Ministry of Science and Technology, Taiwan, under Grant NSTC 111-2218-E-A49-021, NSTC 111-2634-F-A49-008, NSTC 111-2221-E-A49-173-MY3, and NSTC 112-2622-8-A49-013-SB.

Data Availability Statement

The data presented in this paper are available upon request from the corresponding author.

Conflicts of Interest

The authors declare no conflict of interest.

References

  1. Nakajima, S. GaN HEMTs for 5G base station applications. In Proceedings of the 2018 IEEE International Electron Devices Meeting (IEDM), San Francisco, CA, USA, 1–5 December 2018; pp. 14.2.1–14.2.4. [Google Scholar]
  2. Yuk, K.; Branner, G.R.; Cui, C. Future directions for GaN in 5G and satellite communications. In Proceedings of the 2017 IEEE 60th International Midwest Symposium on Circuits and Systems (MWSCAS), Boston, MA, USA, 6–9 August 2017; pp. 803–806. [Google Scholar]
  3. Mishra, U.K.; Parikh, P.; Wu, Y.-F. AlGaN/GaN HEMTs-an overview of device operation and applications. Proc. IEEE 2002, 90, 1022–1031. [Google Scholar] [CrossRef]
  4. Tewari, R.C.; Palo, P.; Maiti, J.; Routray, A. GaN-based Radar Micro-Doppler Augmentation for High Accuracy Fall Detection System. In Proceedings of the IECON 2022—48th Annual Conference of the IEEE Industrial Electronics Society, Brussels, Belgium, 17–20 October 2022; pp. 1–6. [Google Scholar]
  5. Sun, R.; Lai, J.; Chen, W.; Zhang, B. GaN Power Integration for High Frequency and High Efficiency Power Applications: A Review. IEEE Access 2020, 8, 15529–15542. [Google Scholar] [CrossRef]
  6. Palacios, T.; Chakraborty, A.; Rajan, S.; Poblenz, C.; Keller, S.; DenBaars, S.P.; Speck, J.S.; Mishra, U.K. High-power AlGaN/GaN HEMTs for Ka-band Applications. IEEE Electron Device Lett. 2005, 26, 781–783. [Google Scholar] [CrossRef]
  7. Wang, Z.; Yang, D.; Cao, J.; Wang, F.; Yao, Y. A novel technology for turn-on voltage reduction of high-performance lateral heterojunction diode with source-gate shorted anode. Superlattices Microstruct. 2019, 125, 144–150. [Google Scholar] [CrossRef]
  8. Wang, Z.; Zhang, Z.; Wang, S.; Chen, C.; Wang, Z.; Yao, Y. Design and Optimization on a Novel High-Performance Ultra-Thin Barrier AlGaN/GaN Power HEMT With Local Charge Compensation Trench. Appl. Sci. 2019, 9, 3054. [Google Scholar] [CrossRef]
  9. Wang, F.; Chen, W.; Sun, R.; Wang, Z.; Zhou, Q.; Zhang, B. An analytical model on the gate control capability in p-GaN Gate AlGaN/GaN high-electron-mobility transistors considering buffer acceptor traps. J. Phys. D Appl. Phys. 2020, 54, 095107. [Google Scholar] [CrossRef]
  10. Matsunami, H. State-of-the-art wide band-gap semiconductors for power electronic devices. In Proceedings of the International Meeting for Future of Electron Devices, Kyoto, Japan, 26–28 July 2004; pp. 21–22. [Google Scholar]
  11. Flack, T.J.; Pushpakaran, B.N.; Bayne, S.B. GaN Technology for Power Electronic Applications: A Review. J. Electron. Mater. 2016, 45, 2673–2682. [Google Scholar] [CrossRef]
  12. Khandelwal, S.; Goyal, N.; Fjeldly, T.A. A Physics-Based Analytical Model for 2DEG Charge Density in AlGaN/GaN HEMT devices. IEEE Trans. Electron Devices 2011, 58, 3622–3625. [Google Scholar] [CrossRef]
  13. Miranda Calero, J.A.; Rituerto-Gonzalez, E.; Luis-Mingueza, C.; Canabal, M.F.; Barcenas, A.R.; Lanza-Gutierrez, J.M.; Pelaez-Moreno, C.; Lopez-Ongil, C. Bindi: Affective Internet of Things to Combat Gender-Based Violence. IEEE Internet Things J. 2022, 9, 21174–21193. [Google Scholar] [CrossRef]
  14. Ropero, F.; Vaquerizo-Hdez, D.; Muñoz, P.; Barrero, D.F.; R-Moreno, M.D. LARES: An AI-based teleassistance system for emergency home monitoring. Cogn. Syst. Res. 2019, 56, 213–222. [Google Scholar] [CrossRef]
  15. Darwish, A.M.; Boutros, K.; Luo, B.; Huebschman, B.D.; Viveiros, E.; Hung, H.A. AlGaN/GaN Ka-Band 5-W MMIC Amplifier. IEEE Trans. Microw. Theory Tech. 2006, 54, 4456–4463. [Google Scholar] [CrossRef]
  16. Micovic, M.; Brown, D.F.; Regan, D.; Wong, J.; Tang, Y.; Herrault, F.; Santos, D.; Burnham, S.D.; Tai, J.; Prophet, E.; et al. High Frequency GaN HEMTs for RF MMIC Applications. In Proceedings of the 2016 IEEE International Electron Devices Meeting (IEDM), San Francisco, CA, USA, 3–7 December 2016; pp. 3.3.1–3.3.4. [Google Scholar]
  17. Moon, J.S.; Wong, D.; Hu, M.; Hashimoto, P.; Antcliffe, M.; McGuire, C.; Micovic, M.; Willadson, P. 55% PAE and High Power Ka-Band GaN HEMTs with Linearized Transconductance via n+ GaN Source Contact Ledge. IEEE Electron Device Lett. 2008, 29, 834–837. [Google Scholar] [CrossRef]
  18. Nakatani, K.; Yamaguchi, Y.; Komatsuzaki, Y.; Sakata, S.; Shinjo, S.; Yamanaka, K. A Ka-Band High Efficiency Doherty Power Amplifier MMIC using GaN-HEMT for 5G Application. In Proceedings of the 2018 IEEE MTT-S International Microwave Workshop Series on 5G Hardware and System Technologies (IMWS-5G), Dublin, Ireland, 30–31 August 2018; pp. 1–3. [Google Scholar]
  19. Nilchi, J.N.; Liu, R.; Li, S.; Akgul, M.; Rocheleau, T.O.; Nguyen, C.T.-C. Third order intermodulation distortion in capacitive-gap transduced micromechanical filters. In Proceedings of the 2015 Joint Conference of the IEEE International Frequency Control Symposium & the European Frequency and Time Forum, Denver, CO, USA, 12–16 April 2015; pp. 5–10. [Google Scholar]
  20. Toole, B.; Plett, C.; Cloutier, M. RF circuit implications of moderate inversion enhanced linear region in MOSFETs. IEEE Trans. Circuits Syst. I 2004, 51, 319–328. [Google Scholar] [CrossRef]
  21. Vuolevi, J.H.K.; Rahkonen, T.; Manninen, J.P.A. Measurement technique for characterizing memory effects in RF power amplifiers. IEEE Trans. Microw. Theory Tech. 2001, 49, 1383–1389. [Google Scholar] [CrossRef]
  22. Chiu, H.-C.; Fu, J.S.; Chen, C.-W. RF performance of GaAs pHEMT switches with various upper/lower δ-doped ratio designs. Solid-State Electron. 2009, 53, 181–184. [Google Scholar] [CrossRef]
  23. Liu, Z.H.; Ng, G.I.; Arulkumaran, S.; Maung, Y.K.; Teo, K.L.; Foo, S.C.; Sahmuganathan, V. Improved Linearity for Low-Noise Applications in 0.25-μm GaN MISHEMTs Using ALD Al2O3 as Gate Dielectric. IEEE Electron Device Lett. 2010, 31, 803–805. [Google Scholar] [CrossRef]
  24. Guidry, M.; Romanczyk, B.; Li, H.; Ahmadi, E.; Wienecke, S.; Zheng, X.; Keller, S.; Mishra, U.K. Demonstration of 30 GHz OIP3/PDC > 10 dB by MM-wave n-polar deep recess MISHEMTs. In Proceedings of the 2019 14th European Microwave Integrated Circuits Conference (EuMIC), Paris, France, 30 September–1 October 2019; pp. 64–67. [Google Scholar]
  25. Zhang, F.; Zheng, X.; Zhang, H.; Mi, M.; He, Y.; Du, M.; Ma, X.; Hao, Y. Linearity Enhancement of AlGaN/GaN HEMTS with Selective-Area Charge Implantation. IEEE Electron Device Lett. 2022, 43, 1838–1841. [Google Scholar] [CrossRef]
  26. Wang, P.; Ma, X.; Mi, M.; Zhang, M.; Zhu, J.; Zhou, Y.; Wu, S.; Liu, J.; Yang, L.; Hou, B.; et al. Influence of Fin-Like Configuration Parameters on the Linearity of AlGaN/GaN HEMTs. IEEE Trans. Electron Devices 2021, 68, 1563–1569. [Google Scholar] [CrossRef]
  27. Lee, M.-W.; Lin, Y.-C.; Hsu, H.-T.; Gamiz, F.; Chang, E.-Y. Improvement of AlGaN/GaN HEMTs Linearity Using Etched-Fin Gate Structure for Ka Band Applications. Micromachines 2023, 14, 931. [Google Scholar] [CrossRef] [PubMed]
  28. Martinez, R.P.; Munzer, D.J.; Zhou, X.Y.; Shankar, B.; Schmidt, E.-M.; Wildnauer, K.; Wu, B.; Murmann, B.; Chowdhury, S. Best Practices to Quantify Linearity Performance of GaN HEMTs for Power Amplifier Applications. In Proceedings of the 2021 IEEE 8th Workshop on Wide Bandgap Power Devices and Applications (WiPDA), Redondo Beach, CA, USA, 7–11 November 2021; pp. 85–89. [Google Scholar]
  29. Bhardwaj, N.; Upadhyay, B.B.; Parvez, B.; Pohekar, P.; Yadav, Y.; Sahu, A.; Patil, M.; Basak, S.; Sahu, J.; Sabiha, F.S.; et al. Improved RF-DC characteristics and reduced gate leakage in GaN MOS-HEMTs using thermally grown Nb2O5 Gate Dielectric. Phys. Scr. 2022, 98, 015805. [Google Scholar] [CrossRef]
  30. Visvkarma, A.K.; Laishram, R.; Kapoor, S.; Rawal, D.S.; Vinayak, S.; Saxena, M. Improvement in DC and pulse characteristics of AlGaN/GaN HEMT by employing dual metal gate structure. Semicond. Sci. Technol. 2019, 34, 105013. [Google Scholar] [CrossRef]
  31. Kwak, H.-T.; Chang, S.-B.; Kim, H.-J.; Jang, K.-W.; Yoon, H.; Lee, S.-H.; Lim, J.-W.; Kim, H.-S. Operational Improvement of AlGaN/GaN High Electron Mobility Transistor by an inner Field-Plate Structure. Appl. Sci. 2018, 8, 974. [Google Scholar] [CrossRef]
  32. Rawat, A.; Surana, V.K.; Meer, M.; Bhardwaj, N.; Ganguly, S.; Saha, D. Gate Current Reduction and Improved DC/RF Characteristics in GaN-Based MOS-HEMTs Using Thermally Grown TiO2 as a Dielectric. IEEE Trans. Electron Devices 2019, 66, 2557–2562. [Google Scholar] [CrossRef]
  33. Huang, S.; Liu, X.; Wang, X.; Kang, X.; Zhang, J.; Fan, J.; Shi, J.; Wei, K.; Zheng, Y.; Gao, H.; et al. Ultrathin-Barrier AlGaN/GaN Heterostructure: A Recess-Free Technology for Manufacturing High-Performance GaN-on-Si power Devices. IEEE Trans. Electron Devices 2018, 65, 207–214. [Google Scholar] [CrossRef]
  34. Mastro, M.A.; LaRoche, J.R.; Bassim, N.D.; Eddy, C.R. Simulation on the effect of non-uniform strain from the passivation layer on AlGaN/GaN HEMT. Microelectron. J. 2005, 36, 705–711. [Google Scholar] [CrossRef]
  35. Jeon, C.M.; Lee, J.-L. Effects of tensile stress induced by silicon nitride passivation on electrical characteristics of AlGaN/GaN heterostructure field-effect transistors. Appl. Phys. Lett. 2005, 86, 172101. [Google Scholar] [CrossRef]
  36. Lin, Y.C.; Chang, E.Y.; Yamaguchi, H.; Hirayama, Y.; Chang, X.Y.; Chang, C.Y. Device Linearity Comparison of Uniformly Doped and δ-Doped In0.52Al0.48As/In0.6Ga0.4As Metamorphic HEMTs. IEEE Electron Device Lett. 2006, 27, 535–537. [Google Scholar] [CrossRef]
  37. Lin, Y.-C.; Chang, E.Y.; Yamaguchi, H.; Wu, W.-C.; Chang, C.-Y. A δ-Doped InGaP/InGaAs pHEMT With Different Doping Profiles for Device-Linearity Improvement. IEEE Trans. Electron Devices 2007, 54, 1617–1625. [Google Scholar] [CrossRef]
  38. Hsu, C.-H.; Shih, W.-C.; Lin, Y.-C.; Hsu, H.-T.; Hsu, H.-H.; Huang, Y.-X.; Lin, T.-W.; Wu, C.-H.; Wu, W.-H.; Maa, J.-S.; et al. Improved linearity and reliability in GaN metal–oxide–semiconductor high-electron-mobility transistors using nanolaminate La2O3/SiO2 gate dielectric. Jpn. J. Appl. Phys. 2016, 55, 04EG04. [Google Scholar] [CrossRef]
  39. Chiu, H.-C.; Yang, S.-C.; Chien, F.-T.; Chan, Y.-J. Improved device linearity of AlGaAs/InGaAs HFETs by a second mesa etching. IEEE Electron Device Lett. 2002, 23, 1–3. [Google Scholar] [CrossRef]
  40. Lee, P.-H.; Lin, Y.-C.; Hsu, H.-T.; Tsao, Y.-F.; Dee, C.-F.; Su, P.; Chang, E.Y. A Tall Gate Stem GaN HEMT with Improved Power Density and Efficiency at Ka-band. IEEE J. Electron Devices Soc. 2023, 11, 36–42. [Google Scholar] [CrossRef]
  41. Riedmuller, S.; Jacquet, J.-C.; Madel, M.; Chang, C.; Callet, G.; Piotrowicz, S.; Delage, S.; Gruenenpuett, J.; Blanck, H.; Scholz, F. A three-layer resist process for T- and Γ-gates in high electron mobility transistor fabrication. In Proceedings of the 2018 48th European Microwave Conference (EuMC), Madrid, Spain, 23–27 September 2018; pp. 1277–1280. [Google Scholar]
  42. Song, B.; Berardi, S.-R.; Wang, R.; Guo, J.; Hu, Z.; Yue, Y.; Faria, F.; Schuette, M.; Ketterson, A.; Beam, E.; et al. Effect of Fringing Capacitances on the RF Performance of GaN HEMTs with T-Gates. IEEE Trans. Electron Devices 2014, 61, 747–754. [Google Scholar] [CrossRef]
Figure 1. Schematic of the AlGaN/GaN HEMT.
Figure 1. Schematic of the AlGaN/GaN HEMT.
Electronics 12 04336 g001
Figure 2. Process flow diagram of the AlGaN/GaN HEMT.
Figure 2. Process flow diagram of the AlGaN/GaN HEMT.
Electronics 12 04336 g002
Figure 3. IDS-VGS characteristics and Gm of the AlGaN/GaN HEMT with various SiNx thicknesses at VDS = 20 V.
Figure 3. IDS-VGS characteristics and Gm of the AlGaN/GaN HEMT with various SiNx thicknesses at VDS = 20 V.
Electronics 12 04336 g003
Figure 4. (a) |H21| and (b) MSG/MAG versus frequency for AlGaN/GaN HEMTs with different SiNx thicknesses.
Figure 4. (a) |H21| and (b) MSG/MAG versus frequency for AlGaN/GaN HEMTs with different SiNx thicknesses.
Electronics 12 04336 g004
Figure 5. SiNx thicknesses of (a) 150 nm, (b) 200 nm, and (c) 250 nm for the 4 × 50 μm device’s power performance at 28 GHz.
Figure 5. SiNx thicknesses of (a) 150 nm, (b) 200 nm, and (c) 250 nm for the 4 × 50 μm device’s power performance at 28 GHz.
Electronics 12 04336 g005
Figure 6. Two-tone measurement results at 28 GHz for the 4 × 50 μm devices with SiNx thicknesses of (a) 150 nm, (b) 200 nm, and (c) 250 nm.
Figure 6. Two-tone measurement results at 28 GHz for the 4 × 50 μm devices with SiNx thicknesses of (a) 150 nm, (b) 200 nm, and (c) 250 nm.
Electronics 12 04336 g006
Table 1. DC characteristics of the devices with various SiNx thicknesses at VDS = 20 V.
Table 1. DC characteristics of the devices with various SiNx thicknesses at VDS = 20 V.
ParameterstSiNx
150 nm 200 nm 250 nm
IDSS (mA/mm)766.5861861.5
Gm,max (mS/mm)290.1312.9320.9
Vth (V)−3.1−3.7−3.7
GVS (V)1.01.11.2
a 1 −0.52938−0.47639−0.51950
a 3 −0.25548−0.22635−0.24283
a 3 / a 1 0.482600.475140.46743
a 5 −0.00589−0.00491−0.00528
a 5 / a 1 0.011130.010310.01016
Table 2. The fT and fmax values of the devices with SiNx thicknesses of (a) 150 nm, (b) 200 nm, and (c) 250 nm.
Table 2. The fT and fmax values of the devices with SiNx thicknesses of (a) 150 nm, (b) 200 nm, and (c) 250 nm.
ParameterstSiNx
150 nm200 nm250 nm
fT33.751.953.1
fmax76.9132.9138.9
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content.

Share and Cite

MDPI and ACS Style

Hsu, C.-W.; Lin, Y.-C.; Lee, M.-W.; Chang, E.-Y. Investigation of the Effect of Different SiNx Thicknesses on the Characteristics of AlGaN/GaN High-Electron-Mobility Transistors in Ka-Band. Electronics 2023, 12, 4336. https://doi.org/10.3390/electronics12204336

AMA Style

Hsu C-W, Lin Y-C, Lee M-W, Chang E-Y. Investigation of the Effect of Different SiNx Thicknesses on the Characteristics of AlGaN/GaN High-Electron-Mobility Transistors in Ka-Band. Electronics. 2023; 12(20):4336. https://doi.org/10.3390/electronics12204336

Chicago/Turabian Style

Hsu, Che-Wei, Yueh-Chin Lin, Ming-Wen Lee, and Edward-Yi Chang. 2023. "Investigation of the Effect of Different SiNx Thicknesses on the Characteristics of AlGaN/GaN High-Electron-Mobility Transistors in Ka-Band" Electronics 12, no. 20: 4336. https://doi.org/10.3390/electronics12204336

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.

Article Metrics

Back to TopTop