Article

Modeling the Behavior of CFRP Strengthened Concrete Beams and Columns at Different Temperatures

1
Department of Civil and Environmental Engineering, Wayne State University, Detroit, MI 48202, USA
2
College of Civil Engineering, Fuzhou University, Fuzhou 350108, China
*
Authors to whom correspondence should be addressed.
Fibers 2020, 8(2), 10; https://doi.org/10.3390/fib8020010
Submission received: 3 June 2019 / Revised: 21 January 2020 / Accepted: 23 January 2020 / Published: 10 February 2020

Abstract

:
The bonding of thin fiber-reinforced plastics (FRP) composites on the surface of concrete members has emerged as an effective method to increase both the strength and stiffness of concrete members. Although a large volume of experimental and numerical research has performed on existing concrete structures to increase their load carrying capacity, there appears to be less work reported on simulating the influence of temperature on the behavior of concrete structures. This study intends to examine the effects of changing temperature on the mechanical properties of FRP composites as well as deteriorated composites on the structural performance of FRP bonded concrete structures. The overall approach consists of computations using finite element models to simulate the structural behavior of FRP bonded beams and columns. Three-dimensional-extended finite element modeling X-FEM using ABAQUS-CAE v.6.13 program was performed to explore the influence of temperature of (25 °C, 100 °C and 180 °C) on failure loads of FRP strengthened beams and columns with adhesive material. Additionally, the cohesive traction–separation damage model was use to model the delamination of FRP from the concrete. The flexural strength, mid-span deflection, crack patterns, failure loads, and mode of failure for the tested models were compared with the previous experimental study. The results show that a FEM results were in good agreement with experimental results. The flexural strength decreases with temperature rise for FRP strengthened concrete beams. The high temperature 180 °C has an adverse influence on the compressive strength of the specimens. The way of FRP rupture in the simulation was similar to the mode that was observed during the experimental tests.

1. Introduction

One of the main causes of the deterioration of construction materials is due to external environmental conditions (temperature and humidity) [1]. Prolonged exposure or even short-term exposure to elevated temperatures will often produce irreversible physical and chemical changes within adhesives [1].
Deteriorated structures need repair to ensure proper functioning, and to prolong their usefulness [2]. Intact structures may also need modification because of design or construction errors, or to accommodate changes in use. To address this need, engineers have developed methods of strengthening techniques. Traditional strengthening and retrofitting techniques that use steel and cementitious materials do not always provide the most appropriate solutions [2,3].
During the past decade, a large body of research has been directed towards better understanding the behavior of civil infrastructures employing FRP composites, and for the development of design guidelines. Nevertheless, these studies have generally ignored or marginally evaluated the reaction of structural systems using FRP to the environments, most importantly temperature changes, to which civil engineering structures are subjected [3,4].
Using an extensive array of instruments and field as well as laboratory tests, the short-term and long-term performances of four types of FRP composite bridge decks were recently evaluated [5]. The coefficient of thermal expansion and the level of temperature gradient were found to be higher than those of standard reinforced concrete decks [6]. Lack of attention to detailing and thermal characteristics of individual components as well as the entire FRP deck system can lead to build up of large thermal stresses, which can result in unexpected deformations and damage. To ensure satisfactory performance, thermal behavior and the resulting thermal stresses need to be incorporated into the design and detailing of panel-girder connections, field joints, and face sheet-core connection in sandwich type panels [7]. Temperature variation can effect composite behavior as a result of thermal expansion mismatch (for instance between the fiber and matrix or between the plies of different orientation). Further, the level of residual stress will depend on temperature variations [8].
Performance of FRP strengthened structures depends on the efficiency of the bond [2,9], which is directly affected by the roughness of the surface [2]. Preventive measures must be carried out to assure adequate bonding. For instance, proper substrate preparation and on-site tests should be executed to verify that each resin batch has sufficient bond with the concrete substrate [10]. The bond strength decreases when the temperature increases [1].
This study focuses on the behavior of FRP bonded concrete beams and columns under various temperature environments (room temperature, 100 and 180 °C) (77, 212, and 356 °F), using finite element modelling by ABAQUS-CAE v.6.13 program. We focused on hot temperature environments to investigate the applications of FRP systems in many hot and humid regions around the world.
Finite element analysis numerically models the behavior of structures to corroborate with the experimental data. Finite element analysis, as used in structural engineering, determines the overall behavior of a structure by dividing it into a number of simple elements, each of which has well-defined mechanical and physical properties. When analyzing composite structures using finite elements we need to supply to the software appropriate input data for the material being used. Typically, for composites, we shall need moduli and strength of the single plies that constitute a laminate. Occasionally we may input the laminate properties directly [11].
In recent years, the extended finite element method [12] has emerged as a powerful numerical procedure for the analysis of crack problems. The extended finite element method was developed to ease difficulties in solving problems with localized features that are not efficiently resolved by mesh refinement. One of the initial applications was the modelling of fractures in a material [13]. In this original implementation, discontinuous basis functions are added to standard polynomial basis functions for nodes that belonged to elements that are intersected by a crack to provide a basis that included crack opening displacements [13].

2. Literature Review

Elarbi [2] studied the effects of changing hygrothermal conditioning cycles on the durability performance of FRP strengthened concrete beams and columns. The study encompassed the long term impact of moisture, high temperature (100 °C, 180 °C).
The flexural strength of plain concrete beams changed, due to subjecting to 100 °C temperature, the changes and magnitudes of flexural strength depended on the number of cycles. By exposing to 180 °C, both the flexural and compressive strength decreased and the FRP delamination was the dominant mode of failure for all beam specimens. The presence of humidity has some influence on the strength of concrete beams and columns especially at 180 °C.
Di Tommaso et al. [14] investigated the influence of temperature in three point bending tests at temperatures ranging from −100 °C (−212 °F) up to 40 °C (104 °F). Relative to the failure load at room temperature, decreasing failure loads were found both for increasing and decreasing temperatures. The influence of temperature on small scale three point bending tests was investigated by Klamer et al. [15]. In these tests, an increasing failure load was found with increasing temperatures, until around the glass transition temperature of the adhesive (62 °C or 144 °F). For higher temperatures, a decreasing failure load was found due to the changed type of failure.
Mavalar et al. [16] studied the short-term effects of temperature, moisture, and chloride content on the CFRP adhesion using pull-off tests. They found that the bond strength decreased significantly at high temperatures [1,16]. Tadeu et al. [17] performed several double-lap shear tests on concrete specimens externally bonded with steel plates. The authors noted a significant reduction of the failure load by increasing the temperature and reported failures in the adhesive for temperatures higher than 30 °C (or 86 °F).
Obaidat et al. [18] presented a finite element analysis which was validated against laboratory tests of eight beams. All beams were loaded under four point bending but differed in the length of the carbon fiber reinforced plastic (CFRP) plate. The commercial numerical analysis tool ABAQUS was used. The analyses results demonstrated similar results with the experimental data regarding load–displacement response, crack pattern, and debonding failure mode when the cohesive bond model is used. Mohammadi et al. [19] studied a numerical analysis method using XFEM implemented in ABAQUS to model FRP intermediate crack debonding failure which was started at the tip of a flexural crack in a plain concrete beam specimen. The numerical analysis has given stiffer results compared with experimental results [19].
Therefore, this study will focus on the three-dimensional extended finite element modeling x-FEM (offers significant benefits in the numerical modeling of crack propagation) using ABAQUS-CAE v.6.13 program was performed to explore the influence of temperature of (25, 100, and 180 °C) on failure loads of FRP strengthened beams and columns with adhesive material. Additionally, the cohesive traction–separation damage model was used to model the delamination of FRP from the concrete, and a comparison was made between the numerical results and the experimental results [2].

3. Finite Element Modelling

The three-dimensional nonlinear extended finite element method (X-FEM) has been utilized to model the behavior of concrete beams and columns subjected to different temperatures numerically. The ABQUS CAE finite element software was adopted in this study to simulate and predict the load –displacement response of the strengthened concrete beams and columns at room temperature “RT”, 100 °C, and 180 °C.

3.1. FRP Strengthened Concrete Beams at Room Temperature (RT)

A three-dimensional nonlinear (X-FEM) was created to study the performance of FRP strengthened concrete beams with dimensions of 406 (16″) × 109 (4.3″) × 104 mm (4.1″) (length, width, and height) respectively. The beam was modeled as simply supported over a 305 mm (12″) span and loaded at the middle of the span. The model consisted of two parts, the first part represented the concrete beam while the second part epitomized the FRP sheet. Two types of material properties were input to the ABAQUS-CAE. For the first part (concrete), the section type was selected “deformable”, the shape was chosen “Solid”, and the type was “Extrusion”. The element has been considered as an elastic-isotropic material, and the section was chosen as Solid/Homogenous. The Poisson’s ratio was assumed to be 0.18, and concrete density equal to 2.4 × 10−6 Kg/mm3 (0.0867 lb/in3). The average compressive strength of experimental test results was 38 MPa (5502 psi) after 28 days, The Max. Principal Stress was used of 2.45 MPa (355 psi), and the modulus of elasticity of concrete was 2.92 × 104 MPa (4.23 × 106 psi).
The concrete damaged plasticity “CDP” is one of the most popular concrete models used for simulation of concrete behavior in Abaqus. For a full definition of the CDP model in Abaqus the following obligatory parameters should be input: the ratio fb0/fc0 of biaxial compressive yield stress to uniaxial compressive yield stress, the ratio K of the second stress invariant on the tensile meridian to that on the compressive meridian for the yield function, dilation angle, and the viscosity parameter [20,21] (see Table 1).
For FRP “part 2”, elastic isotropic behavior up to failure was assumed. Poisson’s ratio was assumed to be 0.3. The section was solid and Homogeneous. The mechanical properties of FRP were provided by the manufacture (see Table 2).
The sections were meshed by size of 0.6 for concrete (1856 nodes, 1372 elements) and 0.3 for FRP (1620 nodes, 742 elements), the element type was selected as “3D Stress”, and the mesh controls selected Hex, while the mesh technique has been considered as structured, see Figure 1.
To connect the two parts, the type of constraint that has been used was surface-to-surface contact, the concrete beam was designated as the master surface and the FRP was selected to be the slave surface. Contact bonding is supported in the cohesive behavior option of the contact interaction property, see Table 3 for adhesive properties.
The cohesive traction–separation damage model was use to model the delamination of FRP from the concrete.
For flexural strength, the concrete beam model was tested by center-point loading according to ASTM C293, whereas the effective span length was three times of the beam depth and the distance from the center of the support to the beam edge was 50 mm (2″) each side. The load was applied as a static pressure load and the type of boundary conditions has been selected “displacement/rotation.” One support was considered as a pin and the other is a roller, see Figure 2.

3.2. FRP Strengthened Concrete Beams at 100 °C

The same procedures that were performed to model FRP strengthened concrete beams at RT have been followed to obtain the numerical results of strengthened concrete beams at 100 °C. The modulus of elasticity of concrete at 100 °C was lower than the modulus of elasticity at RT based on the experimental data, see Table 4. Table 5 shows concrete properties at 100 °C.
For contact property, the cohesive behavior was used, see Table 6 adhesive properties at 100 °C.

3.3. FRP Strengthened Concrete Beams at 180 °C

The same procedures that were performed to model FRP strengthened concrete beams at RT and 100 °C have been followed to obtain the numerical results of strengthened concrete beams at 180 °C. As shown in Table 7.
For contact property, the cohesive behavior was used. Table 8 shows adhesive properties at 180 °C.

4. Finite Element Modelling for Columns

Likewise, with some differences to the procedures which have been followed to simulate the FRP strengthened concrete beam, the FRP strengthened column has been treated. A 3D nonlinear extended finite-element analysis of the FRP-strengthened column was carried out using the ABAQUS/CAE.

4.1. FRP Strengthened Concrete Columns at Room Temperature (RT)

The model was divided into two parts. While the first part represented the 3-D cylindrical concrete column with a dimension of 20 mm (8″) height and 10 mm (4″) diameter, the second part dealt with the FRP, see Figure 3. The properties have been selected to be the same as those for the FRP strengthened concrete beam simulation. The damage evaluation has been selected to be the same as those for the FRP strengthened concrete beam simulation. The mesh seed was chosen edge by size 0.4 for FRP (1344 nodes, 640 elements) and 0.69 for concrete (1573 nodes, 1440 elements), see Figure 4. The mesh controls selected as Hex-dominated for FRP and Hex for concrete, while the mesh technique has been considered as structured and the element type was 3-D stress for both concrete and FRP.
To connect the two parts, the type of constraint that has been used was surface-to-surface contact. The concrete column was designated as the master surface, while the FRP has been selected to be the slave surface. Contact bonding is enabled in the cohesive behavior option of the contact interaction property. The load has been selected as a static pressure on the upper surface and the type of boundary conditions at the bottom surface was chosen as the displacement/rotation, see Figure 5.

4.2. FRP Strengthened Concrete Columns at 100 °C

The same procedures that were performed to model FRP strengthened concrete columns at RT have been followed to obtain the numerical results of strengthened concrete columns at 100 °C. The modulus of elasticity of concrete at 100 °C was lower than the modulus of elasticity at RT based on the experimental data, see Table 4. Table 5 shows concrete properties at 100 °C. For adhesive properties at 100 °C, see Table 6.

4.3. FRP Strengthened Concrete Columns at 180 °C

The same procedures that were performed to model FRP strengthened concrete columns at RT and 100 °C have been followed to obtain the numerical results of strengthened concrete column at 180 °C. Table 7 shows concrete properties at 180 °C. The adhesive properties at 180 °C are shown in Table 8.

5. Finite Element Analysis Results and Discussion

In this section, the behavior of FRP strengthened concrete beams and columns are discussed and the results were compared with the experimental investigations [2]. The extended finite element method was used to model the behavior of those elements numerically.

5.1. FRP Strengthened Concrete Beams at Room Temperature (RT)

By running the ABQUS-CAE software, the load started to increase by steps and the section began to deform until failure. The concrete crack began at the lowest point of the concrete beam almost at the center and propagated upward, followed by the delamination of the FRP and finally the FRP ruptured. The sequence of failure in the simulation was similar to that of the experimental tests, see Figure 6.
The events of simulation loadings were depicted in Figure 7a. All loading stages are shown in Figure 7b.
As shown in Figure 7, the first concrete crack started when the external load reached 40.75% of the peak load and FRP delamination started when the external load reached 95.07% of the peak load. While the first rupture of CFRP started when the external load reached 99.63% of the peak load, the Max. Principal stress of CFRP reached the input 456 MPa (66,000 psi) at rupture.
By comparing the simulated and experimental flexural load and mid-span deflection of FRP strengthened concrete beams at RT, the experimental results of flexural load were about 27% less than the numerical results, which means the finite element model has been successful in prediction FRP strengthened concrete beam failure load.
The maximum principal stress of concrete reached the input 2.813 MPa (408 psi) at crack, and then gradually increased until the peak load. The failure changed above the FRP from failure in the concrete near the interface with the adhesive to failure exactly in the interface in between the concrete and the adhesive.

5.2. FRP Strengthened Concrete Beams at 100 °C

The events of simulation loadings were depicted in Figure 8a. All loading stages were shown in Figure 8b.
As shown in Figure 8, the first concrete crack started when the external load reached 40.75% of the peak load. There is no rupture of FRP, and FRP delamination started when the external load reached 95.73% of the peak load.
Similarly, when compared the simulated and experimental flexural load and mid-span deflection of FRP strengthened concrete beams at 100 °C, the experimental results of flexural load were about 6% less than the numerical results, which means the finite element model has been successful in prediction FRP strengthened concrete beam failure load. The Max. Principal stress of concrete reached the input Max. Principal stress of concrete 3.047 MPa (442 psi) at crack, then gradually increased until the peak load. The cohesive strength decreases when the temperature increases. See Table 3 and Table 6.
The failure changed the above FRP transition temperature from failure in the concrete near the interface with the adhesive to failure exactly in the interface in between the concrete and the adhesive.

5.3. FRP Strengthened Concrete Beams at 180 °C

The events of simulation loadings were depicted in Figure 9a. All loading stages are shown in Figure 9b.
As demonstrated in Figure 9, the first concrete crack started when the external load reached 41.88% of the peak load. There is no rupture of FRP, and the FRP delamination started when the external load reached 96.24% of the peak load.
Likewise, when compared the simulated and experimental flexural load and mid-span deflection of FRP strengthened concrete beams at 180 °C, the experimental results of flexural load were about 20% less than the numerical results, which means the finite element model has been successful in prediction FRP strengthened concrete beam failure load.
The cohesive strength decreases when the temperature increases see Table 3, Table 6 and Table 8. The failure changed above the FRP transition temperature from failure in the concrete near the interface with the adhesive to failure exactly in the interface in between the concrete and the adhesive.
The maximum principal stress of concrete reached the input Max. Principal stress of concrete 2.813 MPa (408 psi) at crack, then gradually increase until the peak load. Because after the onset of the crack in concrete, stress at the crack tip intends to go infinite and this is known as stress singularity at the crack tip. Therefore, in our simulations, we predict larger max principal stress values than input.
When the first crack shows up on the concrete surface and starts to spread, the FRP strengthening sheet tries to prevent crack propagation. As a result of this resistance, an extremely large max principle stress values will generate. See Table 9 for the comparison of failure load and first rupture beginning for FRP strengthened concrete beams at RT, 100 °C and 180 °C.
We noted that the flexural strength decreases with temperature rise for FRP strengthened concrete beams. The maximum flexural load of 100 °C decreased about 1% for the maximum flexural load of RT. The maximum flexural load of 180 °C decreased about 2% for the maximum flexural load of RT.

5.4. FRP Strengthened Concrete Columns at Room Temperature (RT)

By running the ABQUS-CAE software, the pressure began to increase by steps until the failure occurred. Figure 10 shows the crack pattern at peak load. The way of FRP rupture in the simulation was similar to the mode that was observed during the experimental tests (Figure 11).
At RT, the crack of CFRP started at 96.94% of the peak load. By comparing the simulated and experimental compressive load and mid-span deflection of FRP strengthened concrete columns at RT, the numerical results of compressive load was about 0.99 % less than experimental results, which means the finite element model has been successful in prediction FRP strengthened concrete column failure load.
At 100 °C, the crack of concrete started first, and after that, at the end of load (100% load), the crack of CFRP occurred. The cohesive strength decreases when the temperature increases see Table 3 and Table 6. The failure changed under the FRP transition temperature from failure in the concrete near the interface with the adhesive to failure exactly in the interface in between the concrete and the adhesive. As well as, when the simulated and experimental compressive load and mid-span deflection of FRP strengthened concrete columns at 100 °C were compared, the experimental results of compressive load was about 0.61% less than numerical results, which means the finite element model has been successful in prediction FRP strengthened concrete column failure load.
At 180 °C, the crack of concrete started first, after that at 97.48% of the peak load the crack of CFRP started. For the cohesive strength decreases when the temperature increases, see Table 3, Table 6 and Table 8. The failure changed under the FRP transition temperature from failure in the concrete near the interface with the adhesive to failure exactly in the interface in between the concrete and the adhesive. When compared the simulated and experimental compressive load and mid-span deflection of FRP strengthened concrete columns at 180 °C, the numerical results of compressive load was about 7% less than experimental results, which means the finite element model has been successful in the prediction of FRP strengthened concrete column failure load. The Table 10 shows the comparison of failure load and first rupture beginning for FRP strengthened concrete columns at RT, 100 °C and 180 °C.
The maximum compressive load of 100 °C increased about 27% for the maximum compressive load of RT. The maximum compressive load of 180 °C decreased about 39% for the maximum compressive load of RT. This is the same as the experimental results [2]. This concludes that the high temperature 180 °C has an adverse influence on the compressive strength of the specimens.

6. Conclusions

The following conclusions can be drawn from this research:
(1)
The FE results are in generally agreement with the experimental results for all temperatures. The maximum discrepancy was 27%.
(2)
At room temperature, the FRP strengthened beams showed predominately flexural cracks in concrete, followed by a brief FRP delamination prior to FRP rupture. The first rupture of FRP started when the external load reached 99.63% of the peak load.
(3)
When the temperature is raised to 100 °C and 180 °C, the FRP strengthened beams showed predominately flexural cracks in concrete, followed by a brief FRP delamination. As the temperature rises, a delay of FRP delamination has been observed.
(a)
The maximum flexural load of 100 °C decreased about 1% for the maximum flexural load of RT, these results suggest that the FRP strengthened concrete beams at 100 °C, flexural strength weaker than FRP strengthened concrete beams at RT.
(b)
The maximum flexural load of 180 °C decreased about 2% for the maximum flexural load of RT. These results suggest that the FRP strengthened concrete beams at 180 °C, flexural strength weaker than FRP strengthened concrete beams at RT and 100 °C.
(c)
This concludes that the flexural strength decreases with temperature rise for FRP strengthened concrete beams.
(4)
The FRP strengthened columns showed compression cracks in concrete and FRP rupture. The crack of FRP started at 96.94% of the peak load at room temperature. At the end of load (100% load), the crack of FRP occurred when the temperature is raised to 100 °C. While at 180 °C the crack of CFRP started at 97.48% of the peak load. The crack of FRP increased expansion at 180 °C than 100 °C, in the way of FRP rupture in the simulation was similar to the mode that was observed during the experimental tests.
(a)
The maximum compressive load of 100 °C increased about 27% for the maximum compressive load of RT. These results suggest that the FRP strengthened concrete columns at 100 °C, compressive strength stronger than FRP strengthened concrete columns at RT.
(b)
The maximum compressive load of 180 °C decreased about 39% for the maximum compressive load of RT. This is the same as the experimental results [2]. This concludes that the high temperature 180 °C has an adversely influence on the compressive strength of the specimens.
(5)
The thickness of FRP wrapping was 0.25 mm (0.01 in) in this study. I recommend in future, use thick of FRP wrapping more than 0.25 mm (0.01 in) for beams and columns to withstand high temperature (100 °C and 180 °C).
(a) Also, it should be noted that the above mentioned findings are based on the cohesive behavior formulation (the cohesive traction–separation damage model) was use to the characterization of damage evaluation at the interface between concrete and FRP. In future, the virtual crack closure technique (VCCT) that is also available in the ABAQUS-CAE is recommended to be utilized and compared to the results obtained from the cohesive behavior formulation.

Author Contributions

Conceptualization, B.G., and H.-C.W.; Methodology, B.G., and H.-C.W.; Software, B.G.; Formal Analysis, B.G.; Investigation, H.-C.W.; Experiments; A.E. and H.-C.W.; Writing, B.G. All authors have read and agreed to the published version of the manuscript.

Funding

This research received no external funding.

Conflicts of Interest

The authors declare no conflict of interest.

References

  1. Banea, M.D.; da Silva, L.F.M. Adhesively Bonded Joints in Composite Materials: An overview. Available online: https://journals.sagepub.com/doi/pdf/10.1243/14644207JMDA219 (accessed on 28 January 2020).
  2. Elarbi, A. Durability Performance of FRP Strengthened Concrete Beams and Columns Exposed to Hydrothermal Environment. Ph.D. Dissertation, Wayne State University, Detroit, MI, USA, 2011. [Google Scholar]
  3. Elarbi, A.; Wu, H.-C. Flexural Behavior of Epoxy under Accelerated Hygrothermal Conditions. Fibers 2017, 5, 25. [Google Scholar] [CrossRef] [Green Version]
  4. Foster, S.K.; Bisby, L.A. Fire Survivability of External Bonded FRP Strengthening Systems. J. Compos. Constr. 2008, 12, 553–561. [Google Scholar] [CrossRef]
  5. Taljsten, B. FRP Strengthening of Existing Concrete Structures; Design Guidelines; Lulea University Printing Office: Lulea, Sweden, 2002. [Google Scholar]
  6. Park, S. Durability of Adhesive Joints Between Concrete and FRP Reinforcement in Aggressive Environments. Ph.D. Dissertation, The University of Texas at Austin, Austin, TX, USA, August 2005. [Google Scholar]
  7. Vpgel, H.; Svecova, D. Thermal Compatibility and Bond Strength of FRP Reinforcement in Prestressed Concrete Applications. J. Compos. Constr. 2007, 11, 459–468. [Google Scholar]
  8. Gheorghiu, C.; Labossiere, P.; Raiche, A. Environmental Fatigue Static Behavior of RC Beams with Carbon-Fiber-Reinforced Polymer. J. Compos. Constr. 2004, 8. [Google Scholar] [CrossRef]
  9. Bond of Reinforcement in Concrete; State-of-art Report, Federation International du béton; The International Federation for Structural Concrete: Lausanne, Switzerland, 2000; ISBN 2-88394-050-9.
  10. Fyfe Product Data Sheet: Tyfo_ S Saturant Epoxy, Fyfe Co. LLC. 2011. Available online: http://www.fyfeco.com/products/pdf/tyfosepoxy.pdf (accessed on 28 January 2020).
  11. Matthews, F.L.; Davies, G.A.O.; Hitchings, D.; Soutis, C. Finite Element Modeling of Composite Materials and Structures; Woodhead Publishing Ltd.: Sawston, UK, 2000. [Google Scholar]
  12. Moës, N.; Dolbow, J.; Belytschko, T. A Finite Element Method for Crack Growth without Remeshing. Inter. J. Numerical Methods Eng. 1999, 46, 131–150. [Google Scholar] [CrossRef]
  13. Extended Finite Element Method. Available online: http://en.wikipedia.org/wiki/Extended_finite_element_method (accessed on 28 January 2020).
  14. Di Tommaso, A.; Neubauer, U.; Pantuso, A.; Rostasy, F.S. Behavior of Adhesively Bonded Concrete-CFRP Joints at Low and High Temperatures. Mech. Compos. Mater. 2001, 37, 327–338. [Google Scholar] [CrossRef]
  15. Klamer, E.L.; Hordijk, D.A.; Kleinman, C.S. Debonding of CFRP Laminates Externally Bonded to Concrete Specimens at Low and High Temperatures. In Proceedings of the third International Conference on FRP Composites in Civil Engineering, Miami, FL, USA, 13–15 December 2006; pp. 35–38. [Google Scholar]
  16. Malvar, L.J.; Joshi, N.R.; Beran, J.A.; Novinson, T. Environmental Effects on The Short-Term Bond of Carbon Fiber-Reinforced Polymer CFRP Composites. J Compos. Constr. 2003, 7, 58–63. [Google Scholar] [CrossRef]
  17. Tadeu, A.J.B.; Branco, F.J.F.G. Shear Tests of Steel Plates Epoxy-Bonded to Concrete under Temperature. J. Mater. Civ. Eng. 2000, 12, 74–80. [Google Scholar] [CrossRef]
  18. Obaidat, Y.; Heyden, S.; Dahlblom, O. The Effect of CFRP and CFRP/Concrete Interface Models When Modelling Retrofitted RC Beams with FEM. Compos. Struct. 2010, 92, 1391–1398. [Google Scholar] [CrossRef]
  19. Mohammadi, T.; Wan, B.; Harries, K. Intermediate Crack Debonding Model of FRP Strengthened Concrete Beams Using XFEM. In Proceedings of the Simulia Community Conference, Vienna, Austria, 22 May 2013. [Google Scholar]
  20. Finite Element Analysis Lecture#3; Class Notes, Abaqus Software; Civil Engineering Department, Lawrence Technology University: Southfield, MI, USA, 2010.
  21. Michal, S.; Andrzej, W. Calibration of the CDP model parameters in Abaqus. In Proceedings of the World Congress on Advances in Structural Engineering and Mechanics (ASEM15), Incheon, Korea, 25–29 August 2015. [Google Scholar]
  22. Mikamia, C.; Wu, H.-C.; Elarbi, A. Effect of Hot Temperature on Pull-Off Strength of FRP Bonded Concrete. Constr. Build. Mater. 2015, 91, 180–186. [Google Scholar] [CrossRef]
  23. Dri, F.; Restrepo, D. Characterization of the Mode I Fracture Energy of Adhesive Joints; Course Materials CE 595—Project 2; Civil Engineering Department, Purdue University: West Lafayette, IN, USA, 2011. [Google Scholar]
  24. Finite Element Analysis Lecture#5; Class Notes, Abaqus Software; Civil Engineering Department, Lawrence Technology University: Southfield, MI, USA, 2010.
  25. Ezekiel, S.; Xiao, R.; Chin, C. Constitutive Model for Compressive Strength and Elastic Modulus for Concrete under Elevated Temperature. In Proceedings of the Structures Congress 2013: Bridging Your Passion with Your Profession, Pittsburgh, PL, USA, 2–4 May 2013; pp. 2916–2925. [Google Scholar]
  26. Guo, Z.; Shi, X. Experiment and Calculation of Reinforced Concrete at Elevated Temperatures; Elsevier Inc.: Amsterdam, The Netherlands, 2011. [Google Scholar]
  27. Venkatesh, K. Properties of Concrete at Elevated Temperatures; Michigan State University: East Lansing, MI, USA, 2014. [Google Scholar]
  28. Advanced Materials Epibond® 100 A/B High-Temperature Epoxy Structural Adhesive. Available online: http://www.huntsman.com/corporate/Media%20Library/a_MC4EE584E6EFA7273E040EBCD2C6B19E9/Innovation_MC4EE584E960B7273E040EBCD2C6B19E9/New%20HighPerformance_ME4D57E08A6F79FC2E040EBCD2B6B3510/files/Epibond%20100%20AB_US_e.pdf (accessed on 28 January 2020).
Figure 1. Mesh of concrete beam and FRP strengthening sheet. (a) Mesh of concrete by size (0.6); (b) Mesh of FRP by size (0.3).
Figure 1. Mesh of concrete beam and FRP strengthening sheet. (a) Mesh of concrete by size (0.6); (b) Mesh of FRP by size (0.3).
Fibers 08 00010 g001
Figure 2. Load and boundary conditions of FRP strengthened concrete beam model. (a) Static Pressure Load; (b) Boundary Conditions.
Figure 2. Load and boundary conditions of FRP strengthened concrete beam model. (a) Static Pressure Load; (b) Boundary Conditions.
Fibers 08 00010 g002
Figure 3. 3-D strengthened concrete column model.
Figure 3. 3-D strengthened concrete column model.
Fibers 08 00010 g003
Figure 4. Mesh of the FRP concrete column model.
Figure 4. Mesh of the FRP concrete column model.
Fibers 08 00010 g004
Figure 5. Load and boundary conditions of FRP strengthened column model. (a) Mesh of concrete by size; (b) Mesh of FRP by size.
Figure 5. Load and boundary conditions of FRP strengthened column model. (a) Mesh of concrete by size; (b) Mesh of FRP by size.
Fibers 08 00010 g005
Figure 6. Concrete flexural crack, FRP rupture and delamination at experimental tests. Elarbi, 2011 [2].
Figure 6. Concrete flexural crack, FRP rupture and delamination at experimental tests. Elarbi, 2011 [2].
Fibers 08 00010 g006aFibers 08 00010 g006b
Figure 7. Numerical flexural response of FRP strengthened concrete beams and the stages of concrete crack at RT. (a) The events of simulation loadings; (b) The stages of concrete crack.
Figure 7. Numerical flexural response of FRP strengthened concrete beams and the stages of concrete crack at RT. (a) The events of simulation loadings; (b) The stages of concrete crack.
Fibers 08 00010 g007aFibers 08 00010 g007b
Figure 8. Numerical flexural response of FRP strengthened concrete beams and the stages of concrete crack at 100 °C. (a) The events of simulation loadings; (b) The stages of concrete crack.
Figure 8. Numerical flexural response of FRP strengthened concrete beams and the stages of concrete crack at 100 °C. (a) The events of simulation loadings; (b) The stages of concrete crack.
Fibers 08 00010 g008aFibers 08 00010 g008b
Figure 9. Numerical flexural response of FRP strengthened concrete beams and the stages of concrete crack at 180 °C. (a) The events of simulation loadings; (b) The stages of concrete crack.
Figure 9. Numerical flexural response of FRP strengthened concrete beams and the stages of concrete crack at 180 °C. (a) The events of simulation loadings; (b) The stages of concrete crack.
Fibers 08 00010 g009aFibers 08 00010 g009b
Figure 10. Crack propagation of FRP strengthened concrete column at peak load (RT).
Figure 10. Crack propagation of FRP strengthened concrete column at peak load (RT).
Fibers 08 00010 g010
Figure 11. FRP rupture at experimental tests. Elarbi, 2011 [2].
Figure 11. FRP rupture at experimental tests. Elarbi, 2011 [2].
Fibers 08 00010 g011
Table 1. CDP model parameters. (Class notes. Finite Element Analysis Lecture#3. Lawrence Tech. University, 2010 [20]. Michal and Andrzej, 2015 [21]).
Table 1. CDP model parameters. (Class notes. Finite Element Analysis Lecture#3. Lawrence Tech. University, 2010 [20]. Michal and Andrzej, 2015 [21]).
The ParameterThe Value
Dilation angle [degrees]35
Viscosity parameter0
Eccentricity0.1
fb0/fc01.16
K0.67
Table 2. SikaWrap Hex 113C carbon fiber fabric properties. Elarbi, 2011 [2].
Table 2. SikaWrap Hex 113C carbon fiber fabric properties. Elarbi, 2011 [2].
Typical DataSikaWrap Hex 113C Carbon Fiber
ColorBlack
Primary fiber direction0°/90° (bi-directional)
Weight per square yard196 g/m2 (5.7 oz)
Fiber Properties
Tensile Strength3450 MPa (5 × 105 psi)
Tensile Modulus230,000 MPa (33.4 × 106 psi)
Elongation1.5%
Density1.8 g/cc (0.065 lbs./in3)
Normal Thickness-
Cured Laminate Properties Design Values *
Tensile Strength 456 MPa (66,000 psi)
Tensile modulus41,400 MPa (6.0 × 106 psi)
Elongation at breaks1.2%
Thickness0.25 mm (0.01 in)
* Cured laminate properties with Sikadur Hex 300 Epoxy. Properties after standard post cure 21–24 °C (70–75 °F) for 5 days, then 48 hours at 60 °C (140 °F).
Table 3. Adhesive Properties.
Table 3. Adhesive Properties.
The PropertyThe Value
E: Young’s Modulus of adhesive17.24 GPa
(2.5 × 106 psi)
Elarbi, 2011 [2]
G: Shear Modulus of adhesive0.665 GPa
(96,450.1 psi)
Obaidat et al., 2010 [18]
t: Thickness of adhesive0.1 mm (0.004 in)Estimated
Stiffness CoefficientsKnn = E/t = 6.25 × 108
Kss = G/t = 2.411 × 107
Ktt = G/t = 2.411 × 107
Cohesive Strength6 MPa (870.23 psi)
Mikamia et al., 2015 [22]
Shear Strength2.84 MPa (406.11 psi)τmax = 1.46 Ga 0.165 fct 1.033 Obaidat et al., 2010 [18]
= 1.46 (0.665 0.165) 2.03 1.033
fct is concrete tensile strength
= 0.33 fc’=2.03 MPa
G: Fracture Energy91.8 g/mm (5.14 lb/in)
(Estimated)
= (12 P2 a2) / (E h3 B3) Dri and Restrepo, 2011 [23]
Where P is maximum experimental load, a corresponds to the precrack length, h is the height of the sample, and B is the width of the samples.
Table 4. Elastic properties for concrete (temperature dependent). (Class notes. Finite Element Analysis Lecture#5. Lawrence Tech. University, 2010 [24]).
Table 4. Elastic properties for concrete (temperature dependent). (Class notes. Finite Element Analysis Lecture#5. Lawrence Tech. University, 2010 [24]).
Young’s Modulus N/m2Poisson’s RatioTemperature (°C)
3.49 × 10100.220
3.14 × 10100.2200
2.79 × 10100.2400
Table 5. Concrete Properties at 100 °C.
Table 5. Concrete Properties at 100 °C.
The PropertyThe Value
E100 Young’s Modulus of concrete2.8 × 104 MPa (4062000 psi) (Table 4)
No change in compressive strength (fc’) (Ezekiel, et al., 2013 [25]. Guo and Shi, 2011 [26]. Venkatesh, 2014 [27])38 MPa (5502 psi)
No change in Max. Principal Stress (Ezekiel, et al., 2013 [25]. Guo and Shi, 2011 [26]. Venkatesh, 2014 [27])2.45 MPa (355 psi)
Table 6. Adhesive properties at 100 °C.
Table 6. Adhesive properties at 100 °C.
The PropertyThe Value
E100: Young’s Modulus of adhesive14.3 GPa
(2.075 × 106 psi) Elarbi, 2011 [2]
G100: Shear Modulus of adhesive425.6 MPa
(61728.05 psi) Advanced Materials Epibond® 100 A/B High-temperature Epoxy Structural Adhesive. Available online: [28]
t: Thickness of adhesive0.1 mm (0.004 in) Estimated
Stiffness CoefficientsKnn = E/t = 5.187 × 108
Kss = G/t = 1.5432 × 107
Ktt = G/t = 1.5432 × 107
Cohesive Strength1.2 MPa (174.04 psi) Mikamia et al., 2015 [22]
Shear Strength2.64 MPa (382.89 psi)τmax = 1.46 Ga 0.165 fct 1.033 Obaidat et al., 2010 [18]
= 1.46 (0.4256 0.165) 2.03 1.033
= 2.64 MPa (382.89 psi)
Fracture Energy (G)70.7 g/mm (3.96 lb/in)
(Estimated)
= (12 P2 a2)/(E h3 B3) Dri and Restrepo, 2011 [23]
Where P is maximum experimental load 100 °C, a is correspond to the precrack length 100 °C, h is the height of the samples, and B is the width of the sample.
Table 7. Concrete Properties at 180 °C.
Table 7. Concrete Properties at 180 °C.
The PropertyThe Value
E180 Young’s Modulus of concrete 2.67 × 104 MPa (3,873,000 psi) (Table 4)
No change in compressive strength (fc’) (Ezekiel, et al., 2013 [25]. Guo and Shi, 2011 [26]. Venkatesh, 2014 [27])38 MPa (5502 psi)
No change in Max. Principal Stress (Ezekiel, et al., 2013 [25]. Guo and Shi, 2011 [26]. Venkatesh, 2014 [27])2.45 MPa (355 psi)
Table 8. Adhesive Properties at 180 °C.
Table 8. Adhesive Properties at 180 °C.
The PropertyThe Value
E180: Young’s Modulus of adhesive9825 MPa
(1.425 × 106 psi) Elarbi, 2011 [2]
G180: Shear Modulus of adhesive219.4 MPa
(31,828.52 psi) Advanced Materials Epibond® 100 A/B High-temperature Epoxy Structural Adhesive. Available online: [28]
t: Thickness of adhesive0.1 mm (0.004 in)Estimated
Stiffness CoefficientsKnn = E/t = 3.563 × 108
Kss = G/t = 7.95713 × 106
Ktt = G/t = 7.95713 × 106
Cohesive Strength0.8 MPa (116.03 psi) Mikamia et al., 2015 [22]
Shear Strength2.36 MPa (342.29 psi)τmax = 1.46 Ga 0.165 fct 1.033 Obaidat et al., 2010 [18]
= 1.46 (0.21945 0.165) 2.03 1.033
= 2.36 MPa (342.29 psi)
Fracture Energy (G)62.5 g/mm (3.5 lb/in)
(Estimated)
= (12 P2 a2)/(E h3 B3)
Dri and Restrepo, 2011 [23]
Where P is maximum experimental load 180 °C, a is correspond to the precrack length 180 °C, h is the height of the samples, and B is the width of the sample.
Table 9. Comparison of failure load and first rupture beginning for FRP strengthened concrete beams at RT, 100 °C and 180 °C.
Table 9. Comparison of failure load and first rupture beginning for FRP strengthened concrete beams at RT, 100 °C and 180 °C.
Temp °C Peak Load KN, (lbs)First Rupture of FRP Beginning
RT24.52 KN, (5512.6 lbs)99.63% of the peak load
100 °C24.29 KN, (5461 lbs)no rupture
180 °C23.91KN, (5375 lbs)no rupture
Table 10. Comparison of failure load and first rupture beginning for FRP strengthened concrete columns at RT, 100 °C and 180 °C.
Table 10. Comparison of failure load and first rupture beginning for FRP strengthened concrete columns at RT, 100 °C and 180 °C.
Temp °C Peak Load KN, (lbs)First Rupture of FRP Beginning
RT387.54 KN, (87,122.65 lbs)96.94% of the peak load
100 °C491.9 KN, (110,584.1 lbs)at the peak load
180 °C279.49 KN, (62,831.85 lbs)97.48% of the peak load

Share and Cite

MDPI and ACS Style

Gawil, B.; Wu, H.-C.; Elarbi, A. Modeling the Behavior of CFRP Strengthened Concrete Beams and Columns at Different Temperatures. Fibers 2020, 8, 10. https://doi.org/10.3390/fib8020010

AMA Style

Gawil B, Wu H-C, Elarbi A. Modeling the Behavior of CFRP Strengthened Concrete Beams and Columns at Different Temperatures. Fibers. 2020; 8(2):10. https://doi.org/10.3390/fib8020010

Chicago/Turabian Style

Gawil, Bassma, Hwai-Chung Wu, and Abulgasem Elarbi. 2020. "Modeling the Behavior of CFRP Strengthened Concrete Beams and Columns at Different Temperatures" Fibers 8, no. 2: 10. https://doi.org/10.3390/fib8020010

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.

Article Metrics

Back to TopTop