Next Article in Journal
CVD Diamond Growth Enhanced by a Dynamic Magnetic Field
Next Article in Special Issue
Effect of Strain Levels on the Corrosion Resistance of an Enamel-Coated Steel Rebar
Previous Article in Journal
Fabrication and Properties of Epitaxial VO2 Thin Film on m-Al2O3 Substrate
Previous Article in Special Issue
Investigation of Factors Affecting the Intermediate-Temperature Cracking Resistance of In-Situ Asphalt Mixtures Based on Semi-Circular Bending Test
 
 
Font Type:
Arial Georgia Verdana
Font Size:
Aa Aa Aa
Line Spacing:
Column Width:
Background:
Article

Study on Key Mechanical Parameters of High-Strength Grouting Material

1
Key Laboratory of Advanced Civil Engineering Materials of Ministry of Education, School of Materials Science and Engineering, Tongji University, Shanghai 201804, China
2
China Communications Construction Company Third Harbor Engineering Co., Ltd., Shanghai 200032, China
3
School of Civil Engineering, Suzhou University of Science and Technology, Suzhou 215011, China
*
Author to whom correspondence should be addressed.
Coatings 2023, 13(2), 440; https://doi.org/10.3390/coatings13020440
Submission received: 28 January 2023 / Revised: 13 February 2023 / Accepted: 14 February 2023 / Published: 15 February 2023
(This article belongs to the Special Issue Surface Engineering and Mechanical Properties of Building Materials)

Abstract

:
In order to better design and calculate in infrastructures, it is necessary to clarify the key mechanical parameters of structural materials, such as axial compressive strength, elastic modulus and Poisson’s ratio. High-strength grouting material (HSGM) have begun to be used as structural materials with the development of large and complex structures. A large number of test dates were used to analyze the relationship between the axial compressive strength and the cubic compressive strength of HSGM in the paper. ABAQUS software was used to model the specimens of axial compressive strength, and the strain cloud maps of concrete and HSGM were compared and analyzed. By considering HSGM as two-phase (sand and paste) composites, the relationship between elastic modulus of HSGM and mechanical parameters of component materials was derived, and the test results of the mechanical properties of HSGM with different ratios of sand to cement were used for verification. The test results show that the axial compressive strength of the HSGM is closer to the cubic strength than that of the concrete material, which accords with the finite element analysis results. The elastic modulus of high-strength grouting material conforms to the theoretical derivation of two-phase material. The material composition is one of the main factors affecting the elastic modulus. Poisson’s ratio range of high-strength grouting material is 0.25 ± 0.01 by statistical analysis.

1. Introduction

Cement-based material such as concrete, mortar and grout are widely used in structures because of its good compression performance and low-cost characteristics [1]. With the rapid development of cement-based material technology, high-strength grouting material can have the properties of large fluidity, super early strength and super high strength [2]. It has been a structural material in important engineering foundations such as offshore wind power connecting section not only a grouting material in equipment leveling [3]. The foremost problem is the fact that, due to the lack of data, high-strength grouting material is often considered as concrete in the design of structural foundations [4]. However, the upper limit of the strength range of conventional concrete is 80 MPa, while the final strength of HSGM can reach 120 MPa or higher [5]. In the foundation structure of major engineering such as offshore wind power, the mechanical parameters under pressure are important to the structural design calculation of the grout joint section [6]. The standard values of concrete axial compressive strength and elastic modulus used in design calculation have a certain model formula conversion relationship with the cubic strength, and Poisson’s ratio also has a specified range [7]. There are obvious differences in composition and properties between the high-strength grouting material and concrete. To our knowledge, few studies have yielded mechanical parameters characteristic of HSGM. Therefore, it is urgent to study the key mechanical parameters of high-strength HSGM.
The standard solution to the problem is based on the verification of a model theoretical calculation and analysis of measured data. It is of interest to know whether HSGM still follows the rules of concrete. For our goal, we focus on three problems: what are the characteristics of HSGM axial compressive strength, what are the characteristics of HSGM elastic modulus and what is the range of PIFs genes he HSGM Poisson’s ratio. In this paper, ABAQUS software is used to simulate the grout material and the concrete material test block, and the resulting stress cloud map is analyzed to clarify the difference between HSGM and concrete under axial compressive strength. The difference was verified by testing the axial compressive strength and cubic compressive strength of high-strength grouting material at different ages, and the formula coefficients between them were amended. The results of the elastic modulus and compressive strength are used to verify the elastic model of grout material which was derived by the Mori–Tanaka method and make clear the characteristics of the elastic modulus of grout material. Poisson’s ratio range was calculated by a large number of test results. All these will provide a certain basis for the subsequent engineering design.

2. Experiments

2.1. Materials

The raw materials employed in this work were P.II 52.5 Portland cement from Conch; the main properties of the cement are given in Table 1: fine aggregate from Qingdao China with a fineness modulus is 2.6 and elastic modulus of parent rock is 75 GPa. The main properties of the fine aggregate are given in Table 2: high performance powder water-reducing agent from Yingshan PC100T. The main properties of the water reducing agent are given in Table 3. A physical drawing of cement, fine aggregate and agent are seen in Figure 1.

2.2. Experiment Design

Due to the high compressive strength, the water binder ratio of high-strength grouting materials is generally low; 0.2 was adopted to be the water-binder ratio in this experiment. The water reducing agent content was 0.4% of the cementing material. The apparent density of high-strength grouting material was set at 2400 kg/m3. The dosage of cement, fine aggregate, water and admixture was calculated according to the apparent density, sand binder ratio and water-binder ratio parameters.
The axial compressive strength and cubic compressive strength of HSGM at different ages was tested. Since the structural grout materials have a higher strength at the later stage, in order to improve the data of the low-strength areas, the early strength data were included in the test range, and the strength of the data at each age of 1 day, 2 days, 3 days, 7 days, 14 days and 28 days were collected. There are many factors affecting the strength data of cement-based materials. In order to increase the accuracy of the data and eliminate the influence of strength fluctuations as far as possible, the test was repeated three times to test the axial compressive strength and cubic strength.
Specimens formed by structural grout materials with different sand binder ratios were used to verify the elastic modulus model which was calculated by two-phase theory. The cubic compressive strength and elastic modulus of HSGM with sand binder ratios of 1.75, 1.55, 1.35, 1.15, 0.95, 0.75, 0.55, 0.35 and 0 (pure pulp) at the age of 7 days were tested, respectively. The design of the experiment is given in Table 4.

2.3. Methods

The compressive strength test, elastic modulus test and Poisson’s ratio test procedure was based on “Standard of Test Methods for Physical and Mechanical Properties of Concrete” (GB/T50081-2019) [8]. The loading device was the WHY-2000 electro-hydraulic servo pressure testing machine (Figure 2) manufactured by the Shanghai Hualong Test Instruments Corporation. During the elastic modulus and Poisson’s ratio tests, the strain on the transverse and longitudinal deformation of the specimen was collected by a TDS-530 strain collector.

3. Results and Discussion

3.1. Relationship between Axial Compressive Strength and Cubic Compressive Strength of HSGM

3.1.1. Finite Element Modeling

Based on the ABAQUS software (version STANDARD 2020), the POLARIS-MesoConcrete plug-in was used to accomplish random aggregate production, aggregate group generation and aggregate group random delivery [9]. The maximum particle size of HSGM was 5 mm, and the particle size of concrete aggregate was a continuous gradation from 20 mm. The volume of aggregate in the whole specimen is shown in Table 5. Two-dimensional aggregate models of the axial strength samples of grouting material and concrete were generated respectively. The size of the sample is 300 mm × 100 mm.
As is shown in Figure 3, the green color of the base represents the cement paste, different colored spheres represent aggregate and the size of colored spheres is determined by Table 1.
In keeping with the reality, two steel plates were simulated, respectively, on the upper and lower parts of the specimen. A fixed friction force on the contact surface between steel plate and test block was set as 0.3, as shown in Figure 4. A load of 1100 kN was applied to the upper surface. The strain cloud diagram of HSGM and concrete was obtained through finite element analysis. The local image was cut in the middle of the specimen, as shown in Figure 5.
Concrete strength has strong size effect [10]. According to the Weibull distribution theory, when the size of the specimen increases, the volume of concrete increases, and thus the possibility of defects or large defects increases [11]. The damage and failure of concrete are developed from local stress concentration which is easy to occur in the inherent defects of concrete. The larger the structure size, the higher the possibility of large internal defects, the lower the ultimate compressive strength, and the more significant the size effect. For grout materials, its aggregate particle size is small, and at the same time, its flow performance is good, its gas content is low, so it has good filling property with the bubble and is easy to discharge, and the section structure is dense. The probability of large and serious defects is much lower than that of concrete. According to the strain cloud map (Figure 5), the deformation concentration phenomenon occurs more in the concrete test blocks, but less in the grout material test blocks, which is similar to the theoretical analysis results. The size effect of HSGM is lower than concrete, and the theoretical compressive strength of HSGM of different sizes would be much closer.

3.1.2. Formula for the Relationship between Axial Compressive Strength and Cubic Compressive Strength of HSGM

Figure 6 shows the relationship between the axial compressive strength and cubic compressive strength of concrete, ultra-high performance concrete in other papers [12,13,14,15,16,17,18,19,20,21], and also HSGM from Table 1 in this paper. The axial compressive strength of structural grouting increases with the increase in cubic strength, showing a linear growth trend similar to that of concrete. The axial compressive strength of HSGM is generally higher than that of concrete when the cubic compressive strength is the same. As shown in Figure 7, the coefficients of variation (CV) in different ages are close, which reflected the reliability of the data in this paper.
According to the test results, standard deviation processing was carried out on the strength data to determine the fluctuation range of each data. Since most of the concrete material’s axial compressive strength and cubic compressive strength relationship formula adopted a linear relationship formula, the linear formula was used to fit the axial compressive strength and cubic compressive strength data of high-strength grouting material. We used 18 experimental units from Table 4 No.1 to build a linear regression, each experimental unit have three evaluation according to standard test procedure. The fitting results are shown in Figure 8. The fitting has a very high correlation coefficient which is 0.98, indicating that the fitting formula can well characterize the relationship between the axial compressive strength and the cubic strength of HSGM.
Based on the above data analysis and fitting results, within the range of 60~120 MPa, the standard value formula of axial compressive strength of HSGM can be defined as
f ck = 0.91 f cu , k + 4.1
where fck is the axial compressive strength of HSGM; fcu,k are cubic strength of structural grout material; 0.91 is the reduction coefficient; 4.1 is the correction coefficient.
In general, axial compressive strength is lower than cubic compressive strength in cement-based materials [22]. The gap between axial compressive strength and cubic compressive strength in HSGM is smaller than in concrete, the reduction coefficient of HSGM is higher than concrete which conforms to the finite element simulation results. The model formula of HSGM can better represent the mechanical characteristics of HSGM.

3.2. Relationship between Elastic Modulus and Cubic Compressive Strength of HSGM

3.2.1. Derivation of Elastic Modulus Model

The elastic modulus of HSGM can be deduced by using meso-hierarchy theory based on the distribution and performance parameters of component materials [23]. The grout material can be regarded as the combination of fine aggregate and cement paste. From the meso-level, it is assumed that the fine aggregate and cement paste in the grout material are elastic materials with the same properties in each phase. The bubbles are not considered because there are relatively few bubbles in the grout material. In addition, an interfacial transition zone is not considered because the interfacial transition zone of HSGM is relatively thin and has little effect [24]. The aggregate can be simplified into a sphere because of the aggregate for HSGM is relatively fine and its grain type is round. The aggregate can be seen as a hardened inclusion. The elastic modulus model of structural grout material can be predicted by combining with the theory of multi-phase inclusion.
Mori–Tanaka theory is a widely used multi-phase inclusion theory, which comprehensively considers the influence of distant strain on the interaction between medium [25]. The grout material model uses cement paste as the matrix phase and fine aggregate particles as the inclusion phase. As elastic material, its elastic modulus E, bulk modulus K, shear modulus G and Poisson’s ratio v are related to each other [26]. By inputting the material parameters of aggregate into the model, the model relationship between the elastic modulus of HSGM, the elastic modulus of cement paste and the volume content of aggregate can be obtained:
E c = 9 K c G c 3 K c + G c
where Ec is the elastic modulus of HSGM, GPa; Kc is the volume modulus of HSGM, GPa; Gc is shear modulus of HSGM, GPa.
K c = ( 18.02 + 15.35 V r + 0.221 E m 0.221 V r E m ) E m ( 25.96 25.96 V r + 0.319 E m + 0.375 V r E m )
where Kc is the volume modulus of HSGM, GPa; Vr is aggregate volume content, %; Em is the elastic modulus of cement paste, GPa.
G c = ( 5.764 + 6.236 V r + 0.082 E m 0.082 V r E m ) E m ( 14.52 14.52 V r + 0.206 E m + 0.191 V r E m )
where Gc is shear modulus of HSGM, GPa; Vr is aggregate volume content, %; Em is the elastic modulus of cement paste, GPa.

3.2.2. Test Verification of Elastic Modulus

The volume content of aggregate in HSGM with different sand binder ratios can be calculated by density of material. The volume content and the cubic strength and compressive elastic modulus measured in the same age are shown in Table 6. It can be seen from the data in the table that the cubic strength of the specimen does not change significantly under different aggregate content, and the strength is basically around 115 MPa. This indicates that the volume content of aggregate has little influence on the strength at a low water binder ratio. Although the transition zone increased by the volume content of aggregate, the strength did not decrease, which verifies that the interfacial transition zone is no longer a weak area for HSGM.
The elastic modulus and Poisson’s ratio of pure cement paste obtained in the test were substituted into Formula (5); the model relationship between the elastic modulus of structural grout material and the volume content of aggregate can be written as
E c = 26.25 × V r 2 + 19.57 × V r + 27.36
where Ec is the elastic modulus of structural grout material, GPa; Vr is aggregate volume content, %.
The derived model Formula (5) was placed in the elastic modulus and strength data graphs obtained by testing with different sand binder ratios, as shown in Figure 9.
Figure 9 is the result of 10 experimental units from Table 4, where each experimental unit contains three evaluated units. The average error rate is the average value of error rate contained in all experimental units. The error rate is calculated by the difference between the predicted value and the measured value divides the predicted value. As can be seen from Figure 9, when using the same material and aggregate with different volume contents, the model derived from the material property mechanism is close to the experimental data with the average error rate of just 3%, which proves the accuracy of the elastic modulus model of structural grout materials. At the same time, it also indicates that the elastic modulus is closely related to the aggregate content. The main reason is that the elastic modulus essentially reflects the load-deformation condition of the material at the elastic stage and the content change of its component materials will affect the overall deformation condition. It has been verified in the mechanical test of HSGM, indicating that the component materials of grouting material have a greater influence on the elastic modulus. Therefore, the strength should not be only considered when designing the elastic modulus in structural design, but also the composition and distribution of materials.

3.3. Selection of Poisson’s Ratio

Poisson’s ratio is the ratio of transverse deformation to longitudinal deformation when material is under stress. Most scholars believe that the compressive strength and tensile strength Poisson’s ratio of concrete materials are the same, and Poisson’s ratio is generally closely related to the composition of materials [27,28]. Poisson’s ratio will fluctuate within a range around a certain point. Poisson’s ratio of concrete in the specification is 0.2 [29]. The regression statistical method was adopted to make statistics on the compressive and tensile Poisson’s ratio data obtained in the experiment in this paper, as shown in Table 7. By standard deviation analysis and weighted average calculate, a representative value range was obtained. The calculation formula of sample standard deviation was as follows:
S = ( X i X ¯ ) 2 n 1
where S is the sample standard deviation, Xi is the ith data, X ¯ is the average value of the whole data, and n is the number of the whole samples.
The standard deviation of the compressive Poisson’s ratio is 0.009 and the mean value of the compressive Poisson’s ratio is 0.248. The standard deviation of the tensile Poisson’s ratio is 0.011 and the mean value of the tensile Poisson’s ratio is 0.253. After the combining of compressive and tensile Poisson’s ratios, an average range of 0.25 ± 0.01 can be obtained. Comparing this range with actual data, as show in Figure 10. It can be seen from the figure that more than 95% points fall in this range, which is highly representative.

4. Discussion and Conclusions

The axial compressive strength is important to the main structural force of the whole structure in structural design. Because the axial compressive strength test is not convenient, the cubic compressive strength test is commonly used in the construction process. Concrete is the most commonly used cement-based structure material, and the relationship between the axial compressive strength and cube compressive strength of concrete is relatively clear. HSGM has obvious differences in strength and maximum aggregate particle size to concrete.
The stress concentration phenomenon under pressure in HSGM is significantly less than that in concrete by the finite element analysis of HSGM and concrete axial compressive strength specimens under stress. Test dates show that the axial compressive strength of HSGM is generally higher than that of concrete when the cubic compressive strength is the same; the size effect of HSGM is not as obvious as concrete. The standard value formula between the axial compressive strength and cubic strength of high-strength grouting material can be defined.
The elastic modulus and Poisson’s ratio reflect the deformation characteristics before specimen failure, and they can affect the deformation of the whole structure in the structure design. Under the same pressure, the deformation characteristics of aggregate and paste are different. The Mori–Tanaka model is very successful in predicting the effective properties of two-phase composites.
The relationship model between the elastic modulus of HSGM and the volume content of aggregate is given, by using cement paste as the matrix phase and fine aggregate particles as the inclusion phase with the theory of multi-phase inclusion. The results verify the accuracy of the model with the average error rate of just 3%. In elastic modulus design and calculation, the influence of material composition should be considered in high-strength grouting material.
Based on a large number of Poisson’s ratio data of HSGM, the Poisson’s ratio suitable for structural grout materials is given by statistical analysis, which is 0.25 ± 0.01. Poisson’s ratio covers more than 95% of the measured data, and it is suggested to be used as Poisson’s ratio for HSGM in structure design.

Author Contributions

Conceptualization, Y.Z.; methodology, Y.Z.; software, B.C.; validation, H.Z. and X.Z.; formal analysis, Y.H.; investigation, H.Z.; resources, B.C.; data curation, B.C.; writing—original draft preparation, Y.Z.; writing—review and editing, X.Z.; visualization, H.Z.; supervision, X.Z.; project administration, Y.H. All authors have read and agreed to the published version of the manuscript.

Funding

This research received no external funding.

Institutional Review Board Statement

Not applicable.

Informed Consent Statement

Not applicable.

Data Availability Statement

Not applicable.

Conflicts of Interest

The authors declare no conflict of interest.

References

  1. Su, J.; Yang, Z.; Fang, Z. Size Effect of Concrete Compressive Strength with Different Aggregate Composition. Adv. Concr. Struct. 2009, 400–402, 831–835. [Google Scholar] [CrossRef]
  2. Lu, J.; Chen, J.; Gan, G.; Xu, F. Study on the Preparation of New Type High Capability and None Shrinkage Cement-based Grouting Material. Mater. Rev. 2016, 30, 123–129. [Google Scholar]
  3. Wang, D.; Zhang, Y.; Sun, X.; Gao, J. Development of ultra-high performance cement-based grouting material and its research & application in offshore wind power foundation construction. In Proceedings of the 2020 Fib Symposium: Concrete Structures for Resilient Society, Shanghai, China, 22–24 November 2020; pp. 36–45. [Google Scholar]
  4. Li, Z.X.; Chen, T.; Wang, X. Behavior of flat grouted connections subjected to lateral pressure and vertical load. Constr. Build. Mater. 2019, 212, 329–341. [Google Scholar] [CrossRef]
  5. Fu, T.; Ren, X.Q.; Li, Y.; Wang, K.; Zhu, Z.X. Experimental study on the mechanical behavior of HTRB600E steel sleeve grouting based on UHPC. Case Stud. Constr. Mater. 2022, 17, e01656. [Google Scholar] [CrossRef]
  6. Wang, X.; Chen, T.; Zhao, Q.; Yuan, G.K.; Liu, J.C. Fatigue Evaluation of Grouted Connections under Bending Moment in Offshore Wind Turbines Based on ABAQUS Scripting Interface. Int. J. Steel Struct. 2016, 16, 1149–1159. [Google Scholar] [CrossRef]
  7. Chen, T.; Cao, C.C.; Zhang, C.H.; Wang, X.; Chen, K.; Yuan, G.K. Numerical modeling and parametric analysis of grouted connections under axial loading. Thin-Walled Struct. 2020, 154, 106880. [Google Scholar] [CrossRef]
  8. GB/T50081-2019; Standard of Test Methods for Physical and Mechanical Properties of Concrete. Ministry of Housing and Urban-Rural Development of the PRC, State Administration for Market Regulation: Beijing, China, 2019.
  9. Cheng, S.-H.; Ren, Z.-G.; Li, P.-P.; Shangguan, J.-Y. Numerical Simulation of Concrete Aggregates with Arbitrary Shapes Based on ANSYS/LS-DYNA. J. Wuhan Univ. Technol. 2014, 36, 89–94. [Google Scholar] [CrossRef]
  10. Yang, Q.W.; Du, S.G. Prediction of concrete cubic compressive strength using ANN based size effect model. Comput. Mater. Contin. 2015, 47, 217–236. [Google Scholar]
  11. Kun, Z.; Bai Ru, L.; Xun An, Z.; Yi Hong, W.; Zhan, Q. Research on weibull distribution theory for cubic compressive strength test method of raw earth materials with different curing methods and time. Key Eng. Mater. 2021, 896, 129–140. [Google Scholar] [CrossRef]
  12. Su, J.; Zhang, J.; Zhou, C.B.; Fang, Z. Size Effect on the Cubic Compressive Strength of Reactive Powder Concrete. Rilem Proc. 2016, 105, 585–589. [Google Scholar]
  13. Zhou, J.J.; Pan, J.L.; Leung, C.K.Y.; Li, Z.J. Experimental study on mechanical behavior of high performance concrete under multi-axial compressive stress. Sci. China Technol. Sic. 2014, 57, 2514–2522. [Google Scholar] [CrossRef]
  14. He, X.X.; Lin, S.Y.; Zhen, X.C. Experimental Study on Size Effect of Compressive Strength and Deformation Properties of Large Size Fly Ash Concrete. Key Eng. Mater. 2011, 477, 319–324. [Google Scholar] [CrossRef]
  15. Bandeira, M.V.V.; Zydeck, R.C.; Kosteski, L.E.; Marangon, E. Concrete axial compressive strength with different loading directions and boundary conditions. Materia 2020, 25. [Google Scholar] [CrossRef]
  16. FaghihKhorasani, F.; Kabir, M.Z.; AhmadiNajafabad, M.; Ghavami, K. Predicting compressive stress-strain curves of structural adobe cubes based on Acoustic Emission (AE) hits and Weibull distribution. Int. J. Struct. Integr. 2019, 10, 766–791. [Google Scholar] [CrossRef]
  17. Xiong, M.X.; Liew, J.Y.R.; Wang, Y.B.; Xiong, D.X.; Lai, B.L. Effects of coarse aggregates on physical and mechanical properties of C170/185 ultra-high strength concrete and compressive behaviour of CFST columns. Constr. Build. Mater. 2020, 240, 117967. [Google Scholar] [CrossRef]
  18. Abid, M.; Hou, X.M.; Zheng, W.Z.; Hussain, R.R. Effect of Fibers on High-Temperature Mechanical Behavior and Microstructure of Reactive Powder Concrete. Materials 2019, 12, 329. [Google Scholar] [CrossRef] [Green Version]
  19. Ji, J.; Kang, W.; Jiang, L.Q.; Li, Y.H.; Ren, H.G.; Hao, S.X.; He, L.J.; Lin, Y.B.; Yu, C.Y. Mechanical Behavior of Reactive Powder Concrete Made From Local Material Subjected to Axial Pressure. Front. Mater. 2021, 8, 737646. [Google Scholar] [CrossRef]
  20. Bandeira, M.V.V.; Torre, K.R.L.; Kosteski, L.E.; Marangon, E.; Riera, J.D. Influence of contact friction in compression tests of concrete samples. Constr. Build. Mater. 2022, 317, 125811. [Google Scholar] [CrossRef]
  21. Wu, H.M.; Liu, K.; Yang, F.; Shen, B.; Ma, K.J.; Zhang, J.Y.; Liu, B. Experimental Mechanical Properties and Numerical Simulation of C80 Concrete with Different Contents of Stone Powder. Materials 2022, 15, 3282. [Google Scholar] [CrossRef]
  22. Li, M.; Hao, H.; Cui, J.; Hao, Y.F. Numerical investigation of the failure mechanism of cubic concrete specimens in SHPB tests. Def. Technol 2022, 18, 1–11. [Google Scholar] [CrossRef]
  23. Qiu, Y.R.; Zhang, G.X.; Yin, X.N. Parameters inversion of mortar in concrete considering the hardening process based on meso-mechanics. In Proceedings of the Third Technical Conference on Hydraulic Engineering, Hongkong, China, 13–14 December 2014; pp. 85–92. [Google Scholar]
  24. He, Z.H.; Du, S.G.; Chen, D. Microstructure of ultra high performance concrete containing lithium slag. J. Hazard. Mater. 2018, 353, 35–43. [Google Scholar] [CrossRef] [PubMed]
  25. Yang, C.C.; Huang, R. Double inclusion model for approximate elastic moduli of concrete material. Cem. Concr. Res. 1996, 26, 83–91. [Google Scholar] [CrossRef]
  26. Krishnya, S.; Elakneswaran, Y.; Yoda, Y. Proposing a three-phase model for predicting the mechanical properties of mortar and concrete. Mater. Today Commun. 2021, 29, 102858. [Google Scholar] [CrossRef]
  27. Mina, A.L.; Trezos, K.G.; Petrou, M.F. Optimizing the Mechanical Properties of Ultra-High-Performance Fibre-Reinforced Concrete to Increase Its Resistance to Projectile Impact. Materials 2021, 14, 5098. [Google Scholar] [CrossRef]
  28. Yang, H.Q.; Rao, M.J.; Dong, Y. Influence study of extra-large stone limited size and content on full-graded concrete properties. Constr. Build. Mater. 2016, 127, 774–783. [Google Scholar] [CrossRef]
  29. Aili, A.; Vandamme, M.; Torrenti, J.M.; Masson, B.; Sanahuja, J. Time evolutions of non-aging viscoelastic poisson’s ratio of concrete and implications for creep of C-S-H. Cem. Concr. Res. 2016, 90, 144–161. [Google Scholar] [CrossRef]
Figure 1. Physical drawing of cement (left), fine aggregate (middle) and agent (right).
Figure 1. Physical drawing of cement (left), fine aggregate (middle) and agent (right).
Coatings 13 00440 g001
Figure 2. WHY-2000 electro-hydraulic servo pressure testing machine.
Figure 2. WHY-2000 electro-hydraulic servo pressure testing machine.
Coatings 13 00440 g002
Figure 3. Schematic diagram of aggregate feeding of structural grout material (left) and concrete (right).
Figure 3. Schematic diagram of aggregate feeding of structural grout material (left) and concrete (right).
Coatings 13 00440 g003
Figure 4. Test simulation diagram.
Figure 4. Test simulation diagram.
Coatings 13 00440 g004
Figure 5. HSGM and concrete strain cloud diagrams. (a) HSGM strain cloud diagram, (b) concrete strain cloud diagram.
Figure 5. HSGM and concrete strain cloud diagrams. (a) HSGM strain cloud diagram, (b) concrete strain cloud diagram.
Coatings 13 00440 g005
Figure 6. The relationship between axial strength and cubic strength of grout materials and concrete.
Figure 6. The relationship between axial strength and cubic strength of grout materials and concrete.
Coatings 13 00440 g006
Figure 7. The coefficient of variation in different ages.
Figure 7. The coefficient of variation in different ages.
Coatings 13 00440 g007
Figure 8. Fitting treatment of axial strength and cubic strength of HSGM.
Figure 8. Fitting treatment of axial strength and cubic strength of HSGM.
Coatings 13 00440 g008
Figure 9. Relationship between aggregate content and elastic modulus of structural grout material.
Figure 9. Relationship between aggregate content and elastic modulus of structural grout material.
Coatings 13 00440 g009
Figure 10. Poisson’s ratio distribution range of HSGM.
Figure 10. Poisson’s ratio distribution range of HSGM.
Coatings 13 00440 g010
Table 1. The main properties of cement.
Table 1. The main properties of cement.
-DensitySpecific Surface Area1-Day Compressive Strength3-Day Compressive Strength7-Day Compressive Strength28-Day Compressive Strength
P.II52.5 Portland cement3.02 g/cm3394 m2/kg23.1 MPa39.3 MPa50.8 MPa57.9 MPa
Table 2. The main properties of fine aggregate.
Table 2. The main properties of fine aggregate.
-Apparent DensityBulk DensityTight Bulk DensityStone Powder ContentWater Absorption
Fine aggregate2700 kg/m31490 kg/m31590 kg/m31.5%1.2%
Table 3. The main properties of water reducing agent.
Table 3. The main properties of water reducing agent.
-AppearanceMoisture ContentpHBulk DensityWater Reduction Rate
Water reducing agentPale yellow to white0.5%7.2450 kg/m328%
Table 4. The design of the experiment.
Table 4. The design of the experiment.
No.Water-Binder RatioSand-Binder RatioWater Reducing Agent ContentTest Content
10.21.150.4%Axial compressive strength, cubic compressive strength and Possion’s ratio at 1 day, 2 days, 3 days, 7 days, 14 days and 28 days, three times
20.21.750.4%Elastic modulus and cubic compressive strength at 7 days
30.21.550.4%Elastic modulus and cubic compressive strength at 7 days
40.21.350.4%Elastic modulus, cubic compressive strength and Possion’s ratio at 7 days
50.21.150.4%Elastic modulus and cubic compressive strength at 7 days
60.20.950.4%Elastic modulus, cubic compressive strength and Possion’s ratio at 7 days
70.20.750.4%Elastic modulus and cubic compressive strength at 7 days
80.20.550.4%Elastic modulus and cubic compressive strength at 7 days
90.20.350.4%Elastic modulus and cubic compressive strength at 7 days
100.200.4%Elastic modulus and cubic compressive strength at 7 days
Table 5. The volume of aggregate in HSGM and concrete.
Table 5. The volume of aggregate in HSGM and concrete.
-Less Than 5 mm5 mm–10 mm10 mm–15 mm15 mm–20 mmTotol
Grouting material42%///42%
Concrete20%9%7%6%38%
Table 6. Strength and elastic modulus of grout materials with different sand to paste ratios.
Table 6. Strength and elastic modulus of grout materials with different sand to paste ratios.
No.Sand to Paste RatiosVolume Contents of AggregateCubic Strength/MPaElastic Modulus/GPa
11.7552%114.742.1
21.5549%115.243.5
31.3546%109.142.2
41.1542%115.340.0
50.9537%115.439.3
60.7532%117.637.3
70.5525%116.133.4
80.3518%114.528.5
900%116.527.0
Table 7. Poisson’s ratio statistics of structural grout materials.
Table 7. Poisson’s ratio statistics of structural grout materials.
No.Compressive Poisson’s RatioTensile Poisson’s Ratio
10.2440.271
20.2420.259
30.2410.257
40.2430.256
50.2420.255
60.2400.257
70.2390.243
80.2450.259
90.2420.259
100.2440.271
110.2390.267
120.2510.237
130.2470.259
140.2590.242
150.2480.234
160.2570.246
170.2480.236
180.2540.244
190.2730.240
200.2660.261
average value0.2480.253
standard deviation0.0090.011
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content.

Share and Cite

MDPI and ACS Style

Zhang, Y.; Cao, B.; Zhang, H.; Zhang, X.; He, Y. Study on Key Mechanical Parameters of High-Strength Grouting Material. Coatings 2023, 13, 440. https://doi.org/10.3390/coatings13020440

AMA Style

Zhang Y, Cao B, Zhang H, Zhang X, He Y. Study on Key Mechanical Parameters of High-Strength Grouting Material. Coatings. 2023; 13(2):440. https://doi.org/10.3390/coatings13020440

Chicago/Turabian Style

Zhang, Yueran, Baoyong Cao, Heng Zhang, Xiong Zhang, and Yan He. 2023. "Study on Key Mechanical Parameters of High-Strength Grouting Material" Coatings 13, no. 2: 440. https://doi.org/10.3390/coatings13020440

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.

Article Metrics

Back to TopTop