Next Article in Journal
Metastable Phase Formation, Microstructure, and Dielectric Properties in Plasma-Sprayed Alumina Ceramic Coatings
Previous Article in Journal
Effect of Polyaniline and Graphene Oxide Composite Powders on the Protective Performance of Epoxy Coatings on Magnesium Alloy Surfaces
Previous Article in Special Issue
Quality of Oil- and Wax-Based Surface Finishes on Thermally Modified Oak Wood
 
 
Font Type:
Arial Georgia Verdana
Font Size:
Aa Aa Aa
Line Spacing:
Column Width:
Background:
Article

Preparation and Characterisation of UV-Curable Flame Retardant Wood Coating Containing a Phosphorus Acrylate Monomer

1
NSERC–Canlak Industrial Research Chair in Interior Wood-Product Finishes, Department of Wood and Forest Sciences, Université Laval, Québec City, QC G1V 0A6, Canada
2
CNRS, INRAE, Centrale Lille, UMR 8207-UMET-Unité Matériaux et Transformations, Université de Lille, F-59000 Lille, France
*
Author to whom correspondence should be addressed.
Coatings 2022, 12(12), 1850; https://doi.org/10.3390/coatings12121850
Submission received: 12 October 2022 / Revised: 21 November 2022 / Accepted: 25 November 2022 / Published: 29 November 2022

Abstract

:
The application of a flame retardant coating is an effective solution to enhance the fire retardancy of wood flooring. However, finding the right balance between reducing the flame propagation and good overall coating properties while conserving wood appearance is complex. In order to answer this complex problem, transparent ultraviolet (UV)-curable flame retardant wood coatings were prepared from an acrylate oligomer, an acrylate monomer, and the addition of the tri(acryloyloxyethyl) phosphate (TAEP), a phosphorus-based monomer, at different concentrations in the formulation. The coatings’ photopolymerisation, optical transparency, hardness, water sorption and thermal stability were assessed. The fire behaviour and the adhesion of the coatings applied on the yellow birch panels were evaluated, respectively, using the cone calorimeter and pull-off tests. Scanning electron microscopy (SEM) and energy-dispersive spectroscopy (EDS) analyses were performed on the collected burnt residues to obtain a better understanding of the flame retardancy mechanism. Our study reveals that phosphorus monomer addition improved the coating adhesion and the fire performance of the coated wood without impacting the photopolymerisation. The conversion percentage remained close to 70% with the TAEP addition. The pull-off strength reached 1.12 MPa for the coating with the highest P-monomer content, a value significantly different from the non-flame retarded coating. For the same coating formulation, the peak of heat release rate decreased by 13% and the mass percentage of the residues increased by 37% compared to the reference. However, the flame-retarded coatings displayed a higher hygroscopy. The action in the condensed phase of the phosphorus flame retardant is highlighted in this study.

1. Introduction

With sustainability questions arising in recent decades, wood is more than ever a material of choice for construction. When this renewable resource is supplied from sustainable forests, wood transformation and use are key in the reduction of the energy embodied in building materials. Along with the use of biobased materials, wood constructions provide further energy and greenhouse gas emission savings. In a perspective of limiting global warming, industries are encouraged to replace high-carbon materials with lower-carbon alternatives and when possible, with products based on renewable materials [1]. Hence, using wood instead of steel or cement in the construction sector is one example of emission reduction options. Used since a long time ago for its mechanical properties and visual aspect, wood can be used for both structural and appearance products such as floors, wall panels, ceiling tiles and mouldings [2]. However, the construction industry has to face one limitation of wood: its flammability. To promote their use in non-residential buildings, increasing flame retardancy is thus essential. Different strategies can be employed to improve the fire performance of wood, including the impregnation of flame retardants and the application of flame retardant coatings [3]. In the flooring industry, the second option is usually preferred as it is easier to implement.
Achieving flame retardancy by the application of a flame retardant (FR) coating is mainly dependent on its formulation and the incorporation of FR components. There are different types of flame retardants, the main ones being halogenated compounds, mineral fillers as well as phosphorus- and nitrogen-based compounds. The phosphorus FR have gained interest in recent decades [4]. Phosphorus-based FR may combine a flame retardancy action in the gaseous phase and in the solid phase [5]. Upon phosphorus FR decomposition, various radicals are released including PO• or HPO2• [6]. These are able to react by radical recombination with the highly reactive hydrogen H• and hydroxy OH• radicals present in the flame. Consequently, oxidation reactions in the flame are slowed down. The production of heat being reduced, flame propagation is limited. The action of the phosphorus FR in the solid phase mainly results in its contribution to the char formation by esterification and dehydration [6,7,8]. The generation of acid species upon temperature elevation leads to further reactions with the surrounding polymer matrix and its decomposition by-products. The efficacy of the phosphorus FR is strongly related to its decomposition products’ interaction with the chemical environment in the pyrolysis zone [9].
High-solid-content ultraviolet (UV)-curable coating is the most common technology used in the manufacturing of pre-finished flooring. The finishing system is typically composed of a stain, a tie coat, sealer layers and a topcoat. These coatings are most of the time acrylate based, as this technology offers an overall good price/property balance. The curing is performed within seconds and no drying step is required, offering a time gain compared to waterborne or solvent-borne coatings. The obtained coatings achieve good hardness and excellent chemical resistance [10,11,12].
In this context, the development of P-containing UV-curable coatings to improve the fire performance of wood may represent an interesting approach to widen the use of wood in the construction industry. Few studies deal with transparent UV-curable coatings offering a good flame retardancy of coated wood while still preserving its appearance [13,14,15,16,17,18]. The addition of FR monomers, reactive diluents, is generally the investigated approach. Chambhare, Lokhande et al. studied phosphorus- and nitrogen-based monomer addition in UV-curable wood coating formulations by adding, respectively, the tris-diethanolamine spirocyclic pentaerythritol bisphosphorate and a difunctional (hydroxypropyl methacrylate) piperazine modified with cyclic phosphates [19,20]. They reported an improved fire and water resistance, higher crosslinking density, but a loss of adhesion on wood. However, the flame retardancy has only been assessed on the coating and not on the coating/wood assembly. Naik et al. also reported the preparation of FR wood coating based on phosphorus and silicon monomers [21]. The coating showing a good adhesion and hardness as well as the best UL-94 rating was a blend with both monomers. The authors attributed the enhancement in flame retardancy to the synergistic effect of phosphorous and silicon. A similar study was conducted with a P,N-containing monomer [22]. In both studies, the intrinsic flame retardant properties of the coatings were assessed by the UL-94 test and the limiting oxygen index (LOI) assessment. The synergy of three monomers containing, respectively, P, S and N elements, the triallyl orthophosphate, the pentaerythritol tetrakis (3-mercaptopropionate), and, the N-dimethylacrylamide, was also investigated in another publication [14]. UV-curable coating formulations were applied on Chinese fir wood samples and UL-94 tests were performed. After fire exposure, the authors reported the formation of an intumescent char layer for some coatings thanks to the release of NH3 and CO2, non-flammable gases during the degradation process. In those studies, the mechanical properties of the coatings were not always thoroughly studied. Furthermore, it appears that the flame retardancy characteristic of the coatings is not systematically assessed in the final condition of use, particularly on the wood/coating assembly.
By enlarging the literature review of acrylic-based FR coatings to non-wood applications, a monomer seems particularly interesting, namely the tri(acryloyloxyethyl) phosphate (TAEP). The fire retardancy of the monomer has already been highlighted in several studies [23,24,25]. The synthesis of the trifunctional phosphate acrylate monomer was firstly reported by Liang and Shi [26]. They further studied the thermal degradation of different blends of the TAEP monomer with an epoxy acrylate oligomer or with a polyurethane one [23]. The LOI improved with an increased TAEP content. The highest loading allowed to reach a V0 rating at the UL-94 test for both oligomer mixes. With the thermal degradation of the TAEP phosphate groups, polyphosphoric acids were formed, contributing to the char development. The authors highlighted a particularly effective degradation catalysation action on the epoxy acrylate oligomer. The TAEP addition to an epoxy acrylate oligomer led to a viscosity decrease while promoting the photopolymerisation rates and the thermal stability of the UV-cured resins [24]. The authors reported a V0 rating during the UL-94 test with a TAEP content of 50% in the formulation. TAEP was also used to prepare a silicon-containing hyperbranched polyphosphonate acrylate (HPA), which was then blended with an epoxy acrylate oligomer [25]. In this study, Wang et al. also highlighted the effectiveness of the phosphorus derivative to catalyse the degradation of the oligomer, helping in the formation of a char layer. The transparent HPA-based coatings displayed an improved LOI value and a decreased pHRR and THR. However, the coatings failed to reach a V0 rating for the UL-94 classification with the FR addition. TAEP was also used to develop a FR coating for polyester fabrics [27]. The textiles were plasma-treated before being dipped in the FR formulations and then exposed to UV light. The authors reported an excellent flame retardant property obtained from dipping the fabrics in a blend of TAEP with another FR compound, a 9,10-dihydro-9-oxa-10-phosphaphenanthrene 10-oxide (DOPO) derivative. The improved washing resistance was attributed to the surface plasma treatment.
Using flame-retarded UV-curable finishing layers could be a strategy to achieve the flame retardant performances of flooring. However, there is no solution thoroughly described in the literature that enables to fulfil all the specifications targeted. The aim of this present work is thus to evaluate the use of TAEP in a high-solid-content UV-curable wood sealer coat formulations not only with regard to the fire properties but also the other key performances expected from a coating. High-solid-content UV-curable coatings were thus prepared with different phosphorus monomer percentages. Two layers were applied on wood samples, with a low thickness of 25 μm per coat. The photopolymerisation kinetics were monitored by photo-differential scanning calorimetry (photo-DSC). The coating optical transparency was measured as a wood flooring coating is usually expected to preserve or improve wood appearance. Other coating properties such as hardness, water sorption and thermal stability were also studied. The wood coating adhesion was evaluated by pull-off tests. This study also highlights the flame retardance behaviour of the wood/coating assembly, studied by cone calorimetry. Scanning electron microscopy (SEM) and energy-dispersive spectroscopy (EDS) analyses were performed on the collected residues after the cone calorimetry test to complete the characterisation of the FR coating property.

2. Experimental Section

2.1. Materials

The coatings were prepared with different phosphorus monomer concentrations. Formulations are presented in Table 1. They are based on typical formulations used as sealers for prefinished wood flooring. Both the difunctional epoxy acrylate oligomer (referred as oligomer) and the acrylate monomer tripropylene glycol diacrylate (TPGDA) were supplied by Arkema (Burlington, ON, Canada). The photoinitiator, 2-hydroxy-2-methylpropiophenone (Sigma-Aldrich, Oakville, ON, Canada), was added at 3 wt%. A polybutadiene additive (Cray Valley, Stratford, CT, USA) was used for its defoaming properties at 0.01 wt% in the formulation. All products were graciously provided by Canlak (Daveluyville, QC, Canada).
The phosphorus monomer, TAEP, was prepared by the addition of phosphorus oxychloride to hydroxylethyl acrylate (Sigma-Aldrich, Oakville, ON, Canada) following the synthesis described by Liang and Shi [26]. All the products were used as received without further purification. Proton nuclear magnetic resonance (1H NMR) and Fourier-transform infrared spectroscopy (FTIR) analyses, respectively, displayed in Figures S1 and S2 in the supplementary information, showed the expected structure of TAEP. Its phosphorus concentration was also confirmed by inductively coupled plasma optical emission spectrometry (ICP-OES) analysis.
Yellow birch (Betula alleghaniensis Britt.) 4.5 mm thick lamellas were provided by Mirage (Saint-Georges, Canada). Raw sawn planks were placed in a conditioning room until mass equilibrium. Relative humidity was set at 42% and temperature at 23 °C, allowing wood samples to reach a moisture content of approximately 8%. Wood samples free from knots and defects were used in this study.

2.2. Sample Preparation

Depending on the analysis performed, coatings were either applied on wood samples, steel plates (Type R Q-panels, Q-LAB, Westlake, OH, USA) or on glass panels cleaned with ethanol.
Sample preparation occurred in different stages as shown on Figure 1, with the example of the steps followed prior to the cone calorimeter test. Before coating applications, the wood sample surface was prepared using a 3-step gradual sanding. A first pass was performed at a P-120-grit, then P-150 and the sanding was finalised at P-180. To do so, an automatic sander 36 CCK 1150 (Costa levigatrici S.p.A., Schio, Italy) equipped with paper sanding belts (aluminium oxide type, Abrasifs JJS Inc., Newmarket, ON, Canada) was used.
Prepared formulations were homogenised using a spatula and placed in an ultrasonic bath during 15 min for degassing before use. Formulation viscosity was measured with a piston-type viscometer (ViscoLab 4100, Cambridge Applied Systems Inc., Boston, MA, USA) at 23 °C. Coatings were applied on wood samples, glass or steel plates with a 25 µm wire-wound rod (BYK Gardner, Columbia, SC, USA). To be closer to what is performed in the industry, it was applied in two layers, each of 25 µm. Before applying the second layer, the coating surface was lightly sanded with a P-400-grit paper to promote interlayer adhesion. A 4-sided applicator (BYK Gardner, Columbia, SC, USA) was used for the application when a higher film thickness was necessary for characterisation tests. When the free films were required, coatings were applied on glass panels, cured, and then carefully pealed of the substrate with a razor blade.
Curing was performed under a medium-pressure mercury vapour lamp on a conveyor at a 5 m·min−1 speed under atmospheric conditions. Lamp intensity was set at 500 mW·cm−2, corresponding to an energy dose of 430–450 mJ·cm−2 in the UVA range. The intensity and energy doses were measured before and after curing with a Power Puck II radiometer (EIT, Leesburg, VA, USA).

2.3. Study of the Coating Photopolymerisation

The impact of trifunctional phosphorus monomer addition on the curing behaviour was monitored by photo-DSC. A DSC822e differential scanning calorimeter (Mettler Toledo, Columbia, USA) coupled with a Lightningcure LC5 mercury-xenon lamp (Hamamatsu Photonics K.K., Iwata, Japan) was used in order to measure the enthalpies of reaction during photopolymerisation. To ensure repeatability, lamp intensity was verified with a radiometer (C6080-02, Hamamatsu Photonics K.K., Iwata, Japan). Experiments were performed under air atmosphere at 30 °C. A coating drop of 2.5 ± 0.1 mg was centred in an open aluminium pan. The sample was then irradiated for 60 s at 50 mW·cm−2. Each formulation was tested four times. All DSC exotherms were normalised to sample weight. The photopolymerisation exotherms resulting from photo-DSC allow the calculation of Rp, the rate of polymerisation, the unsaturation conversion and tind, the induction time. The induction time corresponds to the necessary time to achieve 1% of conversion. The polymerisation rate Rp and the conversion percentage were calculated according to Equations (1) and (2), respectively. Both depend on Δ H t h e o , the theoretical heat flow for the complete conversion of the acrylate system expressed in J·g−1. For calculations, a value of 86 kJ·mol−1 was taken for the heat of the polymerisation per acrylic unsaturation [28]. d H / d t corresponds to the measured heat flow at time t and Δ H t to the heat flow generated up to time t.
R p = ( d H / d t ) Δ H t h e o
% C o n v e r s i o n = ( Δ H t Δ H t h e o ) × 100

2.4. Characterisation of the Coating

The coating optical transparency was evaluated by transmittance on a Cary 60 ultraviolet–visible (UV–Vis) spectrophotometer (Agilent Technologies, Santa Clara, CA, USA). Analyses were carried out on 100 μm thick free films with a scanning wavelength ranging from 400 to 800 nm and using a medium scanning speed (600 nm·min−1). An approximation of the glass transition temperature (Tg) and the crosslinking density of the cured films were calculated from dynamic mechanical analysis (DMA) measurements, performed on a DMA Q800 supplied by TA Instruments (New Castle, USA). DMA apparatus was operated in a tensile mode with the frequency set at 1 Hz and the amplitude at 10 μm. A force track of 125% was applied. Measurements were performed at a constant heating rate of 3 °C·min−1 in a temperature range from 30 °C to 150 °C. Coating-free films were laser cut in a rectangular shape of 25 mm per 5 mm, with a thickness of approximately 100 μm. Prior to the test, films were dried at 100 °C during 24 h to avoid any influence of entrapped water. Five repetitions were run per coating formulation. The storage modulus (E′) and loss modulus (E″) resulting from the dynamic mechanical analysis allow the calculation of the loss factor (tan δ), defined as the ratio of E″ over E′. The storage modulus (E′) represents the elastic portion, while the loss modulus (E″) characterises the viscous behaviour of the material. In this study, the maximum of the loss factor was used to approximate the glass transition temperature. The crosslinking density was calculated according to Equation (3). E′min corresponds to the minimum of storage modulus expressed in Pa, T is the temperature at the minimum of storage modulus and R refers to the ideal gas constant.
ν L D = E m i n 3 R T  
Pendulum hardness tests were performed according to the standardised test method ASTM D4366-16 using a König pendulum tester (BYK Gardner, Columbia, USA). The pendulum was placed on the coating applied on a glass plate and set at a 6° angle to the coating surface normal. The number of oscillations were recorded during pendulum damping from a 6° to 3° angle. Five replicas per formulations were tested for the calculations of the mean values and standard deviations. Dynamic instrumented indentations were carried out on a Micro-Combi tester (CSM Instruments, Peseux, Switzerland) with a diamond Berkovich indenter calibrated on fumed silica beforehand. The indenter tip was led normal to a coating surface applying a maximum load of 300 mN. The force was gradually applied in 5 s, held during 2 s before being unloaded on a 3 s period. Indentation tests were performed 5 times for each sample, on at least 3 repetitions per formulation. For this test, coatings were applied on steel panels with a thickness of 125 μm. Higher thickness than the attended application is mandatory in order to have an adequate indenter penetration depth. Steel panels were preferred over wood to ensure substrate hardness homogeneity. Water content was determined with an 890 Titrando titrator for volumetric Karl Fischer titrations equipped with the software TiamoTM Light (Metrohm AG, Herisau, Switzerland). Coating flakes with a thickness of 100 μm were dispersed in N,N-dimethylformamide and then placed in an ultrasonic bath for an hour prior to the Karl Fischer titrations. The analyses were performed twice per formulation. To assess the potential influence of adding phosphorus derivatives on the water uptake of the coating films, sorption and desorption isotherms were performed in triplicate on 10 mg film samples with a thickness of 100 μm. Before the experiments, the samples were dried overnight in an oven at 100 °C. Tests were performed on a DVS Adventure water vapour sorption analyser (Surface Measurement Systems, Allentown, USA) at a constant temperature of 25 °C. First, a step at 0% relative humidity (RH) was performed to allow mass stabilisation. Then, RH was increased from 0% to 95% by means of 5% steps and scaled back down using the same increment. The relative humidity of the analysis chamber was maintained until the sample mass percentage varies less than 0.0001% over a 5 min period or the step time exceeds 24 h. Thermogravimetric analyses (TGAs) were performed on a TGA 851e analyser (Mettler Toledo, Greifense, Switzerland). Experiments were carried out under a nitrogen flow (50 mL·min−1) from 25 °C to 800 °C at a heating rate of 10 °C·min−1. To avoid any interaction with the phosphorus derivatives, a sapphire crucible (70 µL) was used. All experiments were performed in triplicate on free 50 μm thick coating films. Characteristic data such as T5%, the temperature corresponding to 5% of degradation, Tmax, the temperatures of the maximum degradation rates and the percentages of residues at 800 °C were determined.

2.5. Characterisation of the Coating Adhesion on Wood

Adhesion was investigated using pull-off tests based on the test method described in the ASTM D4541-17 standard. Aluminium dollies with a diameter of 20 mm were glued on the coating using a two-component epoxy adhesive (Lepage Marine Epoxy, Henkel, Mississauga, ON, Canada). Prior to the glue application, the dolly surface was sanded with a P-150-grit paper and cleaned with a wipe. The same procedure was performed on the coating surface with a finer sanding paper (P-1500-grit). Steel hex nuts (79 g) were placed on dollies during the adhesive curing to ensure an even pressure applied on each sample. After 48 h, the test area around the dolly was scored by means of a dolly cutter, until the wood substrate was reached. This ensures testing the same surface area. Pull-off tests were carried out on a QTest/5 Elite electromechanical test system with a 5 kN load cell (MTS, Eden Prairie, MN, USA) at a 2 mm·min−1 pull rate. The coating tensile strength was calculated according to Equation (4), where Fmax corresponds to the load at fracture (N) and d, to the dolly diameter (mm). Fracture type was visually assessed based on the described method in the ISO 4624:2016 standard. Twenty repetitions per formulation were performed.
σ = 4 F m a x π d 2
The statistical analysis of data was achieved on the software R: a language and environment for statistical (R Foundation for Statistical Computing, Vienna, Austria). Prior to analysis, the normal distribution of residuals was examined as well as the homogeneity of variances to ensure the validity of the analysis. One-way ANOVA was executed to compare the impact of phosphorus monomer addition in the coating formulations on the pull-off strength. The Tukey’s HSD test allowed a pairwise comparison between the group to identify significant differences at a 0.05 level.

2.6. Fire Performance of Coated Wood Samples

The fire behaviour of the treated wood samples was assessed on a dual cone calorimeter (Fire Testing Technology, East Grinstead, UK). Cone calorimeter is a bench-scale test method widely used to assess a material’s fire behaviour. It gives different parameters as the heat release rate, the time to ignition or the mass loss of the combusting material. However, it offers a limited interpretation of a fire scenario as it does not consider flame spreading.
Experiments were carried out on 100 × 100 mm samples placed in the horizontal position. The distance between the sample and the cone heater was set at 25 mm. Heat flux was set at 35 kW·m−2 for the cone calorimeter tests, corresponding to an early developing fire scenario. Such a heat flux is recommended for explanatory testing [29]. It is particularly appropriate to assess flame-retarded polymers as it matches the fire stage in which their action is crucial. Ignition was forced and the test was stopped 120 s after flame extinction. Wood sample backsides were wrapped in aluminium foil before being put in the sample holder. All experiments were performed in quadruplicate. In order to characterise the fire behaviour of the sample, the following data were gathered: the average time to ignition (TTI), the average peak of the heat release rate (pHRR) and the average total heat released (THR).
Cone calorimeter residues were collected and characterised with an Inspect F50 SEM equipped with a field emission gun source (FEI, Hillsboro, OR, USA). Elemental analysis on the residues was performed by means of energy dispersive spectroscopy (Octane Super-A, EDAX-AMETEK, Mahwah, NJ, USA). The acceleration voltage was set at 15 kV. Prior to analysis, all samples were covered with a conductive Au/Pd deposit.

3. Results

3.1. Photopolymerisation

DSC analysis assesses the heat flow of a material as a function of time and temperature compared to a reference. When coupled with a UV lamp, it enables the measurement of different parameters specific to photo-curable systems. Photo-DSC results are presented in Figure 2 and Table 2.
All the rates of polymerisation curves demonstrated a steep increase within a few seconds after the beginning of the irradiation. Then, a rapid decrease in the rate of polymerisation was observed. Such a heat flow or a Rp behaviour was already reported in the literature for the free radical polymerisation of acrylate systems [30,31]. The rate of polymerisation of free radical polymerisation can be divided into different steps. The induction period is followed by the autoacceleration step, also called the Trommsdorff gel effect or the Norrish−Smith effect. Rp drastically increases due to the increasing viscosity of the polymerising system that slows termination reactions [32]. After reaching its maximum, Rp diminishes during the phase of autodeceleration. The propagation is then controlled through diffusion [33]. In this study, Rpmax were in the same range, with a value of 15.3 s−1 for F2 and 16.1 s−1 for the other systems. The conversion percentages were close to 70% for all coating formulations. The conversion percentages being kept in the same range when replacing the TPGDA by the phosphorus monomer demonstrated its active participation in the curing reaction. Thus, TAEP was successfully incorporated in the polymeric network created during the photopolymerisation of F1 and F2 coatings. No major difference in the induction time nor in the maximum heat flow, Hmax, was noticed.
In the literature, a sharp peak in the rate of photopolymerisation was also observed for TAEP containing formulations [34,35]. However, Rpmax varied with the phosphorus monomer content. Tests were performed at 2.4 mW.cm−2 or at a lower irradiance, greatly inferior to the 50 mW.cm−2 used in this study. Such an irradiance was chosen so as to be more realistic to assess the photopolymerisation behaviour for an industrial application. Lower irradiance generates less energy, and hence, the polymerisation rate is slower. Moreover, the gelation effect induced by the trifunctional monomer addition in the system is greater, explaining the difference in the Rpmax value. The literature also reports that Rp tends to increase when the formulation viscosity decreases [36]. The viscosity is an important parameter for UV-curable systems as it affects different properties such as the ease of application, levelling, polymerisation rate and adhesion. In the present study, the viscosity varied significantly between the formulations (Table 2). However, the addition of TAEP, a non-linear phosphorus monomer, even at a high percentage in the formulation, did not affect the UV-curing behaviour.

3.2. Coating Properties

3.2.1. Optical Transparency

Achieving transparency is an important parameter for wood coatings as they are often designed to protect the substrates while keeping their natural aspect. Film transparency was assessed by spectrophotometry on the visible spectrum, between 400 and 800 nm (Figure 3). F0 film was transparent with an 88% transmittance at 600 nm. With the addition of the FR monomer, the F1 and the F2 coatings also exhibited good optical transparency with a transmittance higher than 87% at 600 nm. All coatings preserved wood aspect as shown on Figure S3 in the supplementary information.

3.2.2. Coating Mechanical Properties

All the factors impacting the chain mobility, such as the steric hindrance, the polymer functionality, the nature of the moving segment or the free volume available for motion, will affect the glass transition temperature. Both monomers added in the formulations in this study, TPGDA and TAEP, differ in their backbone structures and their number of acrylate functionalities. Such differences in chemical composition may lead to polymers exhibiting different Tg and crosslinking densities [37].
DMA results are displayed in Figure 4; the storage modulus (E′) and the tan δ curves are shown in Figure S4 of the supplementary information. The glass transition temperature increased along with TAEP loading. Tg reached 75 °C for F2, ten degrees higher than the one of F0. The oligomer supplier indicates a Tg at 51 °C, measured by DSC. The Tg of the TAEP homopolymer is also known (105 °C) as it has already been measured and reported in the literature [34,35]. While the value of Tg increased with the phosphorus monomer percentage in the formulation, the crosslinking densities were in the same range. Given the standard deviation, the crosslinking densities were not considered to be different. The width of the tan δ curves remained constant, evidencing good miscibility between the phosphate monomer and the acrylate monomer, TPGDA, and the epoxy acrylate oligomer.
Hardness refers to an imprecise term since its definition varies in the literature [38]. A broad definition of the surface hardness corresponds to the coating resistance to deformation by means of the indentation or the penetration of a solid object [39,40]. This is the reason why two technics (pendulum and indentation) were used in this study to determine the hardness of the coatings. The results are reported in Figure 5.
The pendulum hardness results exhibited a higher damping property for the coatings containing the phosphorus monomer. The F0 film reached 108 oscillations, while F1 and F2 achieved 89 and 78 oscillations, respectively. Replacing TPGDA by the TAEP monomer led to a change in the viscoelastic properties of the coating. The phosphorus-containing films were able to dissipate the pendulum energy of motion more easily.
Indentation hardness quantifies the coating film ability to resist to the penetration of an indenter. Preliminary tests confirmed that the maximum applied load ensured that the penetration was restricted to the upper part of the coating film. Having an optimal penetration depth guarantees a minimised influence of the substrate mechanical property on the results. The coating film containing only the acrylate monomer attained an instrumented hardness of approximately 65 MPa. With the addition of phosphorus monomer, the capacity to withstand penetration distinctly dropped under 45 MPa for both F1 and F2 formulations. The reduced elastic modulus Er also followed the same trend, decreasing with a higher phosphorus content. Even though the conversion rate as well as the crosslinking density were not affected by the phosphorus monomer addition, a change in mechanical properties was observed. While TAEP had a higher functionality, the presence of the P-monomer brought flexibility to the coating films. The presence of water in the P-containing films was evidenced by further tests. The plasticising effect of the trapped water in the coating film is one possible explanation for their increased flexibility.

3.2.3. Coating Water Sorption

Using phosphorus-containing polymers in a coating may cause some concern. Phosphorus polymers could be sensitive to moisture and in particular, P-O-C linkages present hydrolytic instability [41]. In order to assess the coating water affinity, Karl Fischer titration and dynamic vapour sorption experiments (DVS) measurements (Figure 6) were performed.
Karl Fischer titration quantifies both free and bound water present in the coating film. The coating without P-monomer contained 0.82% of residual water. The water content rose with the phosphorus addition to achieve 1.30% for F2 coating. These results were consistent with the early stage TGA measurements (Figure 7) showing a higher mass decrease for the phosphorus-containing films. This gap in mass loss could be explained by their higher water content released below 150 °C.
DVS measures the quantity of water absorbed by the coating film in a given range of vapour concentrations. For the F0 film, water absorption was limited, and the mass gain reached 1.90% at the highest RH. The F2 sorption isotherm showed a steep increase in high-relative-humidity percentages. Such behaviour, corresponding to a low intake at low pressures followed by an increased in the high pressures, is typical of a Type III isotherm defined in the International Union of Pure and Applied Chemistry nomenclature [42]. F1 displayed a similar water uptake profile to a minor extent, as the mass change at the maximum RH reached 5.98% instead of 15.3% for F2. The F2 desorption isotherm did not return to a null mass change at a 0% RH. The hypothesis was made that the water is still present in the sample. Further energy seemed to be necessary to remove the bound water. This latter was removed prior to the DVS test by heating during the drying stage at 100 °C. F0 showed no hysteresis on the isotherms of sorption and desorption unlike the coating samples containing phosphorus. The mechanism of water uptake was changed with the presence of a P-monomer in the coating. The absence of hysteresis suggested a plausible surface adsorption mechanism with limited to no bulk absorption. Hence, the results displayed the influence of adding phosphorus derivatives on the water uptake of coating films, mainly in the high RH range.
Although those results could appear as a limit for a coating application, the formulated coatings developed in this study are meant for a sealer use. In a complete wood finishing system, they would benefit from a topcoat applied above. This upper protective layer will limit water exchange and would be designed to resist abrasion and scratch. Once integrated in the finishing system, the sealer has a limited contribution to the surface hardness. Further investigations were thus performed on the coatings and the thermal stability was first studied.

3.2.4. Coating Thermogravimetric Analysis

The thermal stability of the coating films as well as the TAEP monomer was investigated by thermogravimetric analysis in an inert atmosphere. The mass loss curves and their derivatives are shown in Figure 7. The main results (T5%, Tmax and the percentages of residues at 800 °C) are featured in Table 3.
The thermal decomposition of the pure monomer TAEP happened in three distinct steps, with maximum degradation rates at approximately 160 °C, 370 °C and 420 °C. A similar behaviour was reported in the literature for the thermogravimetric analysis of TAEP homopolymer in air [26]. Three main decomposition steps were described and assigned to the decomposition of the phosphate groups (from 160 °C to 270 °C), the decomposition of the ester groups (at approximately 330 °C) followed by the decomposition of unstable structures in the char (above 500 °C). In our study, the analyses showed that the pristine coating underwent a three-stage decomposition process, with a first step around 160 °C, and then two overlapping steps between 300 °C and 475 °C. Even though the F0 formulation was more thermally stable under 400 °C compared to F1 and F2, there was no residue at 800 °C. The major F0 degradation range corresponded to a weight loss of approximately 90%, a percentage greatly higher compared to the ones of phosphorus-containing formulations. F1 and F2 coatings also displayed a several stages of decomposition but with better distinguishable steps. F1 coating first had thermal degradation at a higher temperature range followed by another thermal degradation at approximately 420 °C, which corresponds to the final decomposition of the oligomer and the monomer. For both phosphorus-containing coatings, it was observed that the thermal pyrolysis of unstable structures allowed the formation of a stable char above 450 °C. The major mass loss of F2 cured films occurred between 300 °C and 360 °C. The percentage of residue at 800 °C reached 14.7% for F1 and 19.6% for F2.
Thus, adding phosphorus compounds in the formulation shifts the thermal degradation to a lower temperature but leads to the formation of stable residues at 800 °C. The development of a char could be a benefit in terms of fire performance; the formation of such a protective layer was verified with the cone calorimeter tests.

3.3. Coating Adhesion on Wood

Good adhesion between the coating and the wooden substrate is mandatory to ensure good coating properties and durability [39]. Pull-off tests is a common method to assess the coating adhesion to the substrate that provides a quantitative result. The results of the pull-off strength of the different coatings applied on wood are presented in Figure 8. During the tests, only adhesive failure between the substrate and the first coat happened. An increasing phosphorus content in the coating led to an increasing fibre deposit on the dollies after the test. Thus, the cohesive strength of the coatings was good and the phosphorus coatings seemed to offer a better mechanical anchoring with a higher-wood fibres wetting. The adhesion strength also varied with the phosphorus content. Indeed, while the mean value of the adhesion strength of the F0 coating was under 1.00 MPa, it attained 1.01 and 1.12 MPa for F1 and F2, respectively. The statistical analysis conducted on the results revealed a significant difference in adhesion strength between the coating without phosphorus monomer and the one with the highest content. Thus, above a certain P-monomer addition in the formulation, the pull-off strength was slightly enhanced. Phosphorus derivatives are well-known adhesion promoters [43]. For instance, Maege et al. studied the adsorption of phosphorus derivatives on metallic substrates as an anchor to the coating system, offering an improved adhesion [44]. Wang et al. suggested that a phytic acid-based compound enhanced the adhesion of UV-curing coating to metal by the formation of P-O-Fe chemical bonds [45]. Even though the presence of phosphorus additives enhancing the adhesion with wood for coatings or adhesives has been reported in different studies [15,46,47], the mechanism explaining this improvement is not well detailed.
The difference in pull-off test results could be explained by several factors including the limited coating penetration into wood [48] or the UV coating shrinkage through curing [49]. During the photopolymerisation of acrylate systems, the weak intermolecular Van der Waals interactions in the liquid coating are replaced by strong and short covalent bonds between the carbon atoms in the solid film [50]. The distance between carbon atoms is reduced, building up internal stress in the coating. The volume contraction induces a shrinkage that may lead to low coating adhesion and poor mechanical properties [49]. In order to obtain a better understanding, SEM analyses were performed on the sample cross-sections to observe the wood/coating interface (Figure 9). The F0 sample clearly displayed the coating detachment from the wooden substrate in different areas. The interface between the phosphorus coating and wood showed better bonding. The TAEP presence in the formulation seemed to induce lesser coating shrinkage through photopolymerisation, enhancing the coating adhesion.

3.4. Fire Performance of the Coated Wood Samples

Heat release curves are displayed in Figure 10 and key values are summarised in Table 4. All coated panels present a heat release curve with two peaks, similar to what is usually observed in the literature for virgin wood [51]. The first peak is attained before charring. The heat release rate then decreases as a protective layer, i.e. a char, is formed. Then, the HRR curve illustrates the gradual burning through the thickness of the wood sample after the formation of the initial char. Once the carbonaceous protective layer crakes, a second HRR rise happens. The second peak also corresponds to the increased rate of volatile formation prior to the end of the flame burning [52].
F0 coating cracked within a few seconds after exposure to the heat flux. The coating delaminated from the surface, exposing the wooden substrate to the flame. A high first heat release rate peak was rapidly reached for the F0 sample. A second peak was observed attaining a value of 390 kW·m−2. The higher the value of the HHR first peak for the F0 coating compared to the other samples was attributed to the greater organic coating contribution to the burning. The phosphorus coatings also showed some delamination but to a lesser extent compared to F0. This difference in coating adhesion to wood was already highlighted with pull-off tests. A good coating adhesion is critical in the beginning of the cone calorimeter test and decisive for the fire behaviour of the material. Some cracks also appeared on F1 and F2 coating surface after the ignition. Similarly to what was observed for the F0 coating, the HRR curve of F1-coated wood samples presented a first peak but with a lower value, suggesting the formation of a protective char layer. The heat transfer and fuel supply to the flame were limited, slowing down the pyrolysis process. Cracks in the protective layer appeared, allowing the flame to reach the virgin wood. An increase in the pyrolysis then occurred, leading to a second heat release rate rise. For the highest phosphorus-FR-containing film (F2 coating), the curve depression was considerably flattened. It was assumed that the protective layer is formed more efficiently for the F2 sample as a plateau rather than a peak was observed on the HRR curve in the early stage of the test. In the case of phosphorus-containing coatings, the pHRR only reached 340 kW·m−2 and was delayed compared to F0. Adding a phosphorus monomer enhanced the residual mass percentage as well as reduced the THR, suggesting an improved wood charring behaviour. The time to ignition also varied with the FR loading with an upward tendency.
A reduction of 13% in the pHRR could appear as a moderate improvement. However, adding a phosphorus monomer positively affected other parameters such as the percentage of residues after the test. Wang et al. also reported a pHRR decrease of approximately 10% with their best treatment obtained in the cone calorimeter test performed at 50 kW·m−2 [15]. The wood coatings reported in this study contained the following FR at different ratios: a multifunctional bio-mercaptan of castor oil grafted thiol, 2,4,6-trimethyl-2,4,6-trivinylcyclotrisilazane and an organic phosphorus compound. The UV-curable coating was applied at 180 µm (versus 50 µm in the present study) on 4 mm thick Chinese fir samples. The pHRR curve followed a reverse tendency compared to our study, with a higher first peak compared to the second one. Higher pHRR decreases were observed for a non UV-curable waterborne intumescent wood coating [53] or for coating applied on wood with a thicker layer [54]. For the first study, Song et al. obtained a clear pHRR decrease of approximately 40% and a delayed TTI compared to pure wood, a 4 mm thick poplar panel. All the pHRR of the samples treated with the different intumescent coatings ranged from 140 kW·m−2 to 190 kW·m−2 after the cone calorimeter test. In the second study, epoxy coatings were applied on a poplar wood sample at a 5 mm thick layer. The authors reported a pHRR reduction of 20% with the addition of a phosphaphenanthrene-containing epoxy co-curing agent in the coating formulation compared to the epoxy coating reference.
The cone calorimeter residues were collected and analysed to better comprehend the charring mechanism. SEM analyses were performed on the residues collected after the test to confirm the action of phosphate moieties in the condensed phase (Figure 11). The mass percentages of different elements obtained from the EDS analysis performed on the same residues are gathered in Table 5.
F0 residues displayed a very fragile fibrous structure with no visible coating deposit. No charring was observed, only ashes were formed. It is similar to wood sample morphology after being exposed to a flame as reported in the literature [55]. On the contrary, the flame-retarded samples clearly displayed some wooden charred structure demonstrating that a protective mechanism occurred. For both F1 and F2 samples, high temperature-resisting residues of the coating were noticeable. In the case of the F1 sample, a partial delamination of the coating was observed, revealing a thick char underneath. This solid structure is present on the right-hand side of Figure 11b. Fractures in the F1 residues were also visible. They went through the coating and the substrate. F2 residues also displayed a thick char formation. Almost no coating detachment was noticed but cracks were still observed. Interestingly, most of the cracks did not go through the substrate either. Indeed, Figure 11d revealed that most F2 coating fractures were protected by an underneath layer. The F2 burnt sample showed a surface morphology with hollowed areas and trapped bubbles underneath the top layer.
Thus, the presence of a protective layer after the cone calorimetry tests on the residues of wood samples, either coated with F1 or F2 formulation, validates an action of the phosphate moieties in the condensed phase. The TAEP addition to the coating formulation helped the char formation, increasing the mass residue. An insulating barrier is formed, protecting the underneath substrate from fire, and preventing gas exchange between the condensed phase and the flame.
EDS analyses further endorsed the action of phosphorus compounds participating in the char formation. Whereas the analysis of the F0 residues revealed the presence of typical elements found in wood ash, the elemental composition significantly varied when a phosphorus-containing coating was applied on the wood. Misra et al. observed that the wood ash at 600 °C was mainly composed of calcium, potassium and magnesium, apart from carbon and oxygen elements [56]. Phosphorus, sulphur and manganese were also present to a minor extent. Wood decomposition forms calcium carbonate and oxide [57]. High O wt% and Ca wt% for F0 endorsed the presence of calcium derivatives. F1 and F2 surface analysis demonstrated higher C and P contents. The phosphorus coming from the FR coating application was still present in the residues after the cone calorimeter test. As expected, a higher P content was observed for F2 compared to F1. A significant amount of phosphorus induces an active role of the FR in a condensed phase mechanism. It is worth mentioning that even though the P content of area 2 of F0 sample and the one of F1 sample were in the same range, these were not comparable as the percentages of the other elements were completely different. EDS analysis gives the relative elemental composition of a local sample area based on the total detected elements in it. While F0 corresponded to an ashes area with a C content under 15%, the F1 sample charred, resulting in a high C content, above 80%.
We may conclude that a decrease in the pHRR combined with an increase in the residual mass indicates an effective action of the TAEP addition regarding flame retardancy. The cone calorimeter tests along with the observation of the residues also suggested a difference in coating adhesion depending on the phosphorus rate in the formulation. With a higher phosphorus content, the least coating delamination occurred, contributing to the improvement of the fire behaviour of the coated wood.

4. Conclusions

High-solid-content transparent UV-curable coatings were prepared at different TAEP percentages in an acrylate-based formulation. Coatings were applied on wood panels. The photopolymerisation kinetics was monitored by photo-DSC. It was shown that adding the phosphorus monomer did not impact the UV-curing behaviour as the conversion of the acrylate group was in the same range, i.e., over 65%. A change in coating hardness was observed and attributed to the fact that TAEP brought flexibility to the coating films. This study also showed that P-containing coatings displayed a higher water sorption for high relative humidity. The issue related to water affinity could be easily lowered by integrating the formulation as a sealer coat in a prefinished wood flooring system. The presence of the phosphorus monomer at the highest content significantly improved the coating adhesion on the wood. The wood coating fire efficacy was evaluated by cone calorimetry. A decreased pHRR as well as an enhanced residue percentage were obtained for all the phosphorus-containing coatings. SEM and EDS analyses performed on the collected residues confirmed the formation of a solid protective structure and the presence of phosphorus in the flame-retarded samples. The phosphorus FR had an effective action in the condensed phase, improving the fire retardancy of the coated wood. The formulation containing approximately 40% of TAEP clearly displayed the best FR performances compared to the non-FR coating. Furthermore, the major expected properties of a sealer coating were positively assessed. This study thus demonstrates the high potential of phosphorus-containing UV-curable acrylate system to improve the fire behaviour of wood flooring. Further investigations could include the introduction of another FR retardant in the formulation. Nitrogen or silicon compounds have demonstrated a synergistic behaviour along with the phosphorus FR. The F2 coating highlighted in this study could also be of interest for metal coating where TAEP could act as both a flame retardant and an adhesion promoter.

Supplementary Materials

The following supporting information can be downloaded at: https://www.mdpi.com/article/10.3390/coatings12121850/s1. Figure S1. 1H NMR spectrum of tri(acryloyloxyethyl) phosphate (TAEP); Figure S2. FTIR spectrum of tri(acryloyloxyethyl) phosphate (TAEP); Figure S3. Appearance of the coatings applied on wood panels; Figure S4. Storage modulus and tan δ curves resulting from DMA analysis on the coating films.

Author Contributions

Conceptualisation, S.P., F.S., S.D. and V.L.; methodology, S.P., F.S., S.D. and V.L.; software, S.P.; validation, S.P.; formal analysis, S.P.; investigation, S.P.; writing—original draft preparation, S.P.; writing—review and editing, S.P., F.S., S.D. and V.L.; supervision, S.D. and V.L.; project administration, S.D. and V.L.; funding acquisition, V.L. All authors have read and agreed to the published version of the manuscript.

Funding

This work is part of the research program of Natural Sciences and Engineering Research Council of Canada (NSERC) Canlak Industrial Research Chair in Finishes for Interior wood products (CRIF) through programs CRD (Grant No. 500235) and Research Support Program, part 4: Support for International Research and Innovation Initiatives (PSR-SIRII in French, Program No. 2590) subsidised by the Ministry for Economy, Science and Innovation (MESI) of Québec.

Institutional Review Board Statement

Not applicable.

Informed Consent Statement

Not applicable.

Data Availability Statement

The data presented in this study are available upon request from the corresponding author.

Acknowledgments

The authors are grateful to the NSERC-Canlak Industrial Research Chair in Finishes for Interior wood products (CRIF) industrial partners for their help, support, and product supply. The authors would like to acknowledge the help of Suzie Côté and the Research Centre for Advanced Materials (CERMA, Université Laval) for SEM imaging as well as Jenny Lapierre and the SEREX for the Karl Fischer titrations. The authors would also like to thank all the technical team at the Renewable Materials Research Centre (CRMR, Université Laval) and specifically Yves Bédard, Daniel Bourgault and Luc Germain, who provided technical support. The assistance provided by Julia B. Grenier for the phosphorus monomer synthesis was greatly appreciated.

Conflicts of Interest

The authors declare no conflict of interest. The funders had no role in the design of the study; in the collection, analyses or interpretation of data; in the writing of the manuscript, or in the decision to publish the results.

References

  1. De Coninck, H.; Revi, A.; Babiker, M.; Bertoldi, P.; Buckeridge, M.; Cartwright, A.; Dong, W.; Ford, J.; Fuss, S.; Hourcade, J.-C.; et al. Strengthening and Implementing the Global Response. Available online: https://www.ipcc.ch/report/sr15/chapter-4-strengthening-and-implementing-the-global-response/ (accessed on 13 September 2022).
  2. Cobut, A.; Blanchet, P.; Beauregard, R. Prospects for Appearance Wood Products Ecodesign in the Context of Nonresidential Applications. For. Prod. J. 2016, 66, 196–210. [Google Scholar] [CrossRef]
  3. Lowden, L.; Hull, T. Flammability Behaviour of Wood and a Review of the Methods for Its Reduction. Fire Sci. Rev. 2013, 2, 4. [Google Scholar] [CrossRef] [Green Version]
  4. Lu, S.-Y.; Hamerton, I. Recent Developments in the Chemistry of Halogen-Free Flame Retardant Polymers. Prog. Polym. Sci. 2002, 27, 1661–1712. [Google Scholar] [CrossRef]
  5. Joseph, P.; Ebdon, J.R. Phosphorus-Based Flame Retardants. In Fire Retardancy of Polymeric Materials; Wilkie, C.A., Morgan, A.B., Eds.; CRC Press: Boca Raton, FL, USA, 2010; pp. 107–127. ISBN 978-1-4200-8399-6. [Google Scholar]
  6. Schartel, B. Phosphorus-Based Flame Retardancy Mechanisms—Old Hat or a Starting Point for Future Development? Materials 2010, 3, 4710–4745. [Google Scholar] [CrossRef] [Green Version]
  7. Levchik, S.V.; Weil, E.D. Developments in Phosphorus Flame Retardants. In Advances in Fire Retardant Materials; Woodhead Publishing Series in Textiles; Elsevier Science: Amsterdam, The Netherlands, 2008; pp. 41–66. ISBN 978-1-84569-507-1. [Google Scholar]
  8. Lyons, J.W. Mechanisms of Fire Retardation with Phosphorus Compounds: Some Speculation. J. Fire Flammabl. 1970, 1, 302–311. [Google Scholar]
  9. Braun, U.; Balabanovich, A.I.; Schartel, B.; Knoll, U.; Artner, J.; Ciesielski, M.; Döring, M.; Perez, R.; Sandler, J.K.W.; Altstädt, V.; et al. Influence of the Oxidation State of Phosphorus on the Decomposition and Fire Behaviour of Flame-Retarded Epoxy Resin Composites. Polymer 2006, 47, 8495–8508. [Google Scholar] [CrossRef]
  10. Decker, C. High-Performance UV-Cured Acrylic Coatings. In New Developments in Coatings Technology; Zarras, P., Wood, T., Richey, B., Benicewicz, B.C., Eds.; American Chemical Society: Washington, DC, USA, 2007; Volume 962, pp. 176–189. ISBN 978-0-8412-3963-0. [Google Scholar]
  11. Decker, C. Kinetic Study and New Applications of UV Radiation Curing. Macromol. Rapid Commun. 2002, 23, 1067–1093. [Google Scholar] [CrossRef]
  12. Müller, B.; Poth, U. Radiation Curing. In Coatings Formulation: An International Textbook; European coatings tech files; Vincentz Network: Hanover, Germany, 2011; pp. 242–255. ISBN 978-3-86630-872-5. [Google Scholar]
  13. Ma, G.; Wang, X.; Cai, W.; Ma, C.; Wang, X.; Zhu, Y.; Kan, Y.; Xing, W.; Hu, Y. Preparation and Study on Nitrogen- and Phosphorus- Containing Fire Resistant Coatings for Wood by UV-Cured Methods. Front. Mater. 2022, 9, 851754. [Google Scholar] [CrossRef]
  14. Wang, T.; Liu, T.; Ma, T.; Li, L.; Wang, Q.; Guo, C. Study on Degradation of Phosphorus and Nitrogen Composite UV-Cured Flame Retardant Coating on Wood Surface. Prog. Org. Coat. 2018, 124, 240–248. [Google Scholar] [CrossRef]
  15. Wang, T.; Li, L.; Cao, Y.; Wang, Q.; Guo, C. Preparation and Flame Retardancy of Castor Oil Based UV-Cured Flame Retardant Coating Containing P/Si/S on Wood Surface. Ind. Crops Prod. 2019, 130, 562–570. [Google Scholar] [CrossRef]
  16. Huang, Y.; Ma, T.; Li, L.; Wang, Q.; Guo, C. Facile Synthesis and Construction of Renewable, Waterborne and Flame-Retardant UV-Curable Coatings in Wood Surface. Prog. Org. Coat. 2022, 172, 107104. [Google Scholar] [CrossRef]
  17. Ma, T.; Li, L.; Liu, Z.; Zhang, J.; Guo, C.; Wang, Q. A Facile Strategy to Construct Vegetable Oil-Based, Fire-Retardant, Transparent and Mussel Adhesive Intumescent Coating for Wood Substrates. Ind. Crops Prod. 2020, 154, 112628. [Google Scholar] [CrossRef]
  18. Mali, P.P.; Pawar, N.S.; Sonawane, N.S.; Patil, V.; Patil, R. UV Curable Flame Retardant Coating: A Novel Synthetic Approach of Trispiperazido Phosphate Based Reactive Diluent. Pigment Resin Technol. 2021, 50, 271–283. [Google Scholar] [CrossRef]
  19. Chambhare, S.U.; Lokhande, G.P.; Jagtap, R.N. UV-Curable Behavior of Phosphorus- and Nitrogen-Based Reactive Diluent for Epoxy Acrylate Oligomer Used for Flame-Retardant Wood Coating. J. Coat. Technol. Res. 2016, 13, 703–714. [Google Scholar] [CrossRef]
  20. Lokhande, G.; Chambhare, S.; Jagtap, R. Synthesis and Properties of Phosphate-Based Diacrylate Reactive Diluent Applied to UV-Curable Flame-Retardant Wood Coating. J. Coat. Technol. Res. 2017, 14, 255–266. [Google Scholar] [CrossRef]
  21. Naik, D.; Wazarkar, K.; Sabnis, A. UV-Curable Flame-Retardant Coatings Based on Phosphorous and Silicon Containing Oligomers. J. Coat. Technol. Res. 2019, 16, 733–743. [Google Scholar] [CrossRef]
  22. Mulge, S.; Mestry, S.; Naik, D.; Mhaske, S. Phosphorus-Containing Reactive Agent for UV-Curable Flame-Retardant Wood Coating. J. Coat. Technol. Res. 2019, 16, 1493–1502. [Google Scholar] [CrossRef]
  23. Liang, H.; Huang, Z.; Shi, W. Different Effects of Tri(Acryloyloxyethyl) Phosphate on the Thermal Degradation of Photopolymerized Epoxy Acrylate and Polyurethane Acrylate Films. J. Appl. Polym. Sci. 2006, 99, 3130–3137. [Google Scholar] [CrossRef]
  24. Yao, C.; Xing, W.; Ma, C.; Song, L.; Hu, Y.; Zhuang, Z. Synthesis of Phytic Acid-Based Monomer for UV-Cured Coating to Improve Fire Safety of PMMA. Prog. Org. Coat. 2020, 140, 105497. [Google Scholar] [CrossRef]
  25. Wang, X.; Xing, W.; Song, L.; Yu, B.; Shi, Y.; Yang, W.; Hu, Y. Flame Retardancy and Thermal Properties of Novel UV-Curing Epoxy Acrylate Coatings Modified by Phosphorus-Containing Hyperbranched Macromonomer. J. Polym. Res. 2013, 20, 165. [Google Scholar] [CrossRef]
  26. Liang, H.; Shi, W. Thermal Behaviour and Degradation Mechanism of Phosphate Di/Triacrylate Used for UV Curable Flame-Retardant Coatings. Polym. Degrad. Stab. 2004, 84, 525–532. [Google Scholar] [CrossRef]
  27. Qi, L.; Wang, B.; Zhang, W.; Yu, B.; Zhou, M.; Hu, Y.; Xing, W. Durable Flame Retardant and Dip-Resistant Coating of Polyester Fabrics by Plasma Surface Treatment and UV-Curing. Prog. Org. Coat. 2022, 172, 107066. [Google Scholar] [CrossRef]
  28. Andrzejewska, E.; Andrzejewski, M. Polymerization Kinetics of Photocurable Acrylic Resins. J. Polym. Sci. Part Polym. Chem. 1998, 36, 665–673. [Google Scholar] [CrossRef]
  29. International Standard Organization. Reaction-to-Fire Tests, Heat Release, Smoke Production and Mass Loss Rate; ISO: Geneva, Switzerland, 2005. [Google Scholar]
  30. Khudyakov, I.V.; Legg, J.C.; Purvis, M.B.; Overton, B.J. Kinetics of Photopolymerization of Acrylates with Functionality of 1−6. Ind. Eng. Chem. Res. 1999, 38, 3353–3359. [Google Scholar] [CrossRef]
  31. Jiang, F.; Drummer, D. Curing Kinetic Analysis of Acrylate Photopolymer for Additive Manufacturing by Photo-DSC. Polymers 2020, 12, 1080. [Google Scholar] [CrossRef]
  32. Norrish, R.G.W.; Smith, R.R. Catalysed polymerization of methyl methacrylate in the liquid phase. Nature 1942, 150, 336–337. [Google Scholar] [CrossRef]
  33. Decker, C. Photoinitiated Crosslinking Polymerisation. Prog. Polym. Sci. 1996, 21, 593–650. [Google Scholar] [CrossRef]
  34. Liang, H.; Asif, A.; Shi, W. Photopolymerization and Thermal Behavior of Phosphate Diacrylate and Triacrylate Used as Reactive-Type Flame-Retardant Monomers in Ultraviolet-Curable Resins. J. Appl. Polym. Sci. 2005, 97, 185–194. [Google Scholar] [CrossRef]
  35. Huang, Z.; Shi, W. Synthesis and Properties of a Novel Hyperbranched Polyphosphate Acrylate Applied to UV Curable Flame Retardant Coatings. Eur. Polym. J. 2007, 43, 1302–1312. [Google Scholar] [CrossRef]
  36. Scranton, A.B.; Bowman, C.N.; Peiffer, R.W. (Eds.) Photopolymerization: Fundamentals and Applications; ACS Symposium Series; American Chemical Society: Washington, DC, USA, 1997; Volume 673, ISBN 978-0-8412-3520-5. [Google Scholar]
  37. Plazek, D.J.; Ngai, K.L. The Glass Temperature. In Physical Properties of Polymers Handbook; Mark, J.E., Ed.; Springer: New York, NY, USA, 2006; pp. 187–215. ISBN 978-0-387-31235-4. [Google Scholar]
  38. Sato, K. The Hardness of Coating Films. Prog. Org. Coat. 1980, 8, 1–18. [Google Scholar] [CrossRef]
  39. Bulian, F.; Graystone, J. Wood Coating: Theory and Practice; Elsevier Science: Amsterdam, The Netherlands, 2009; ISBN-10: 0444528407; ISBN-13: 978-0444528407. [Google Scholar]
  40. Lambourne, R.; Strivens, T.A. Paint and Surface Coatings; Woodhead Publishing Limited: Sawston UK, 1999; ISBN 978-1-85573-348-0. [Google Scholar]
  41. Maiti, S.; Banerjee, S.; Palit, S.K. Phosphorus-Containing Polymers. Prog. Polym. Sci. 1993, 18, 227–261. [Google Scholar] [CrossRef]
  42. Thommes, M.; Kaneko, K.; Neimark, A.V.; Olivier, J.P.; Rodriguez-Reinoso, F.; Rouquerol, J.; Sing, K.S.W. Physisorption of Gases, with Special Reference to the Evaluation of Surface Area and Pore Size Distribution (IUPAC Technical Report). Pure Appl. Chem. 2015, 87, 1051–1069. [Google Scholar] [CrossRef] [Green Version]
  43. Cassidy, P.E.; Yager, B.J. Coupling Agents as Adhesion Promoters. J. Macromol. Sci. Part Rev. Polym. Process. 1971, 1, 1–49. [Google Scholar] [CrossRef]
  44. Maege, I.; Jaehne, E.; Henke, A.; Adler, H.-J.P.; Bram, C.; Jung, C.; Stratmann, M. Self-Assembling Adhesion Promoters for Corrosion Resistant Metal Polymer Interfaces. Prog. Org. Coat. 1998, 34, 1–12. [Google Scholar] [CrossRef]
  45. Wang, X.; Zhang, J.; Liu, J.; Luo, J. Phytic Acid-Based Adhesion Promoter for UV-Curable Coating: High Performance, Low Cost, and Eco-Friendliness. Prog. Org. Coat. 2022, 167, 106834. [Google Scholar] [CrossRef]
  46. Cheng, H.N.; Ford, C.; Dowd, M.K.; He, Z. Effects of Phosphorus-Containing Additives on Soy and Cottonseed Protein as Wood Adhesives. Int. J. Adhes. Adhes. 2017, 77, 51–57. [Google Scholar] [CrossRef] [Green Version]
  47. Zhao, X.; Liang, Z.; Huang, Y.; Hai, Y.; Zhong, X.; Xiao, S.; Jiang, S. Influence of Phytic Acid on Flame Retardancy and Adhesion Performance Enhancement of Poly (Vinyl Alcohol) Hydrogel Coating to Wood Substrate. Prog. Org. Coat. 2021, 161, 106453. [Google Scholar] [CrossRef]
  48. de Moura, L.F.; Hernández, R.E. Evaluation of Varnish Coating Performance for Two Surfacing Methods on Sugar Maple Wood. Wood Fiber Sci. 2005, 37, 355–366. [Google Scholar]
  49. He, Y.; Yao, M.; Nie, J. Shrinkage in UV-Curable Coatings. In Protective Coatings: Film Formation and Properties; Wen, M., Dušek, K., Eds.; Springer International Publishing: Cham, Switzerland, 2017; pp. 195–223. ISBN 978-3-319-51625-7. [Google Scholar]
  50. Park, J.-W.; Shim, G.-S.; Back, J.-H.; Kim, H.-J.; Shin, S.; Hwang, T.-S. Characteristic Shrinkage Evaluation of Photocurable Materials. Polym. Test. 2016, 56, 344–353. [Google Scholar] [CrossRef]
  51. Schartel, B.; Hull, T.R. Development of Fire-Retarded Materials—Interpretation of Cone Calorimeter Data. Fire Mater. 2007, 31, 327–354. [Google Scholar] [CrossRef]
  52. Grexa, O.; Lübke, H. Flammability Parameters of Wood Tested on a Cone Calorimeter. Polym. Degrad. Stab. 2001, 74, 427–432. [Google Scholar] [CrossRef]
  53. Song, F.; Liu, T.; Fan, Q.; Li, D.; Ou, R.; Liu, Z.; Wang, Q. Sustainable, High-Performance, Flame-Retardant Waterborne Wood Coatings via Phytic Acid Based Green Curing Agent for Melamine-Urea-Formaldehyde Resin. Prog. Org. Coat. 2022, 162, 106597. [Google Scholar] [CrossRef]
  54. Li, M.; Hao, X.; Hu, M.; Huang, Y.; Qiu, Y.; Li, L. Synthesis of Bio-Based Flame-Retardant Epoxy Co-Curing Agent and Application in Wood Surface Coating. Prog. Org. Coat. 2022, 167, 106848. [Google Scholar] [CrossRef]
  55. Jiang, J.; Li, J.; Hu, J.; Fan, D. Effect of Nitrogen Phosphorus Flame Retardants on Thermal Degradation of Wood. Constr. Build. Mater. 2010, 24, 2633–2637. [Google Scholar] [CrossRef]
  56. Misra, M.K.; Ragland, K.W.; Baker, A.J. Wood Ash Composition as a Function of Furnace Temperature. Biomass Bioenergy 1993, 4, 103–116. [Google Scholar] [CrossRef]
  57. Etiégni, L.; Campbell, A.G. Physical and Chemical Characteristics of Wood Ash. Bioresour. Technol. 1991, 37, 173–178. [Google Scholar] [CrossRef]
Figure 1. Wood sample preparation for the cone calorimeter test.
Figure 1. Wood sample preparation for the cone calorimeter test.
Coatings 12 01850 g001
Figure 2. Polymerisation rate of the different coatings.
Figure 2. Polymerisation rate of the different coatings.
Coatings 12 01850 g002
Figure 3. UV–Vis transmittance spectra of the coating film.
Figure 3. UV–Vis transmittance spectra of the coating film.
Coatings 12 01850 g003
Figure 4. Crosslinking density and glass transition temperature of the coatings.
Figure 4. Crosslinking density and glass transition temperature of the coatings.
Coatings 12 01850 g004
Figure 5. Pendulum hardness and indentation results of the coating films.
Figure 5. Pendulum hardness and indentation results of the coating films.
Coatings 12 01850 g005
Figure 6. Karl Fischer titration results and, sorption and desorption curves of the coating films. The hollow circles correspond to the sorption step while the filled circles correspond to the desorption one.
Figure 6. Karl Fischer titration results and, sorption and desorption curves of the coating films. The hollow circles correspond to the sorption step while the filled circles correspond to the desorption one.
Coatings 12 01850 g006
Figure 7. Curves of the thermogravimetric analysis performed under nitrogen and their derivatives for the TAEP monomer and the coating films with different phosphorus contents.
Figure 7. Curves of the thermogravimetric analysis performed under nitrogen and their derivatives for the TAEP monomer and the coating films with different phosphorus contents.
Coatings 12 01850 g007
Figure 8. Pull-off strength of the coatings applied on wood. Letters above the bars correspond to the groups determined in the Tukey comparison test after the ANOVA analysis (α = 0.05). Groups having a letter in common are not significantly different.
Figure 8. Pull-off strength of the coatings applied on wood. Letters above the bars correspond to the groups determined in the Tukey comparison test after the ANOVA analysis (α = 0.05). Groups having a letter in common are not significantly different.
Coatings 12 01850 g008
Figure 9. SEM images of the wood/coating interface, F0 (a), F1 (b) and F2 (c). Arrows show coating detachments of few microns wide from wood.
Figure 9. SEM images of the wood/coating interface, F0 (a), F1 (b) and F2 (c). Arrows show coating detachments of few microns wide from wood.
Coatings 12 01850 g009
Figure 10. Cone calorimeter heat release rate curves of the coated wood samples.
Figure 10. Cone calorimeter heat release rate curves of the coated wood samples.
Coatings 12 01850 g010
Figure 11. SEM images of cone calorimeter residues of F0 (a), F1 (b) and F2 (c,d).
Figure 11. SEM images of cone calorimeter residues of F0 (a), F1 (b) and F2 (c,d).
Coatings 12 01850 g011
Table 1. Composition of the UV-curable wood coating formulations.
Table 1. Composition of the UV-curable wood coating formulations.
Raw MaterialF0F1F2
Oligomer47.047.047.0
TPGDA50.030.911.7
TAEP0.019.138.3
Ricon 1300.010.010.01
Photoinitiator3.03.03.0
Table 2. Coating viscosity and photo-DSC results including the induction time, the maximum heat flow, the rate of polymerisation and the unsaturation conversion.
Table 2. Coating viscosity and photo-DSC results including the induction time, the maximum heat flow, the rate of polymerisation and the unsaturation conversion.
FormulationViscosity
(cP, 23 °C)
tind
(s)
Hmax
(W.g−1)
Rpmax
(s−1)
%Conversion
(%)
F06301.06 ± 0.0458 ± 216.1 ± 0.468 ± 3
F18401.10 ± 0.0260 ± 116.1 ± 0.469 ± 1
F212301.13 ± 0.0160 ± 315.3 ± 0.767 ± 2
Table 3. Results of thermogravimetric analysis. T5% corresponds to the temperature at which 5% of the sample mass is lost, Tmax 1, Tmax 2 and Tmax 3 are the temperatures of the degradation rate maxima.
Table 3. Results of thermogravimetric analysis. T5% corresponds to the temperature at which 5% of the sample mass is lost, Tmax 1, Tmax 2 and Tmax 3 are the temperatures of the degradation rate maxima.
FormulationT5%
(°C)
Tmax 1
(°C)
Tmax 2
(°C)
Tmax 3
(°C)
Residue at 800 °C (%)
F02951583714181 ± 1
F119616135742414.7 ± 0.5
F216916833142419.6 ± 0.5
TAEP11313230743630.6 ± 0.2
Table 4. Main cone calorimeter results of the coated wood samples.
Table 4. Main cone calorimeter results of the coated wood samples.
ParameterF0F1F2
Phosphorus coating content * (wt%)0.01.73.4
TTI (s)71 ± 277 ± 990 ± 20
pHRR (kW·m−2)390 ± 10340 ± 10340 ± 10
THR (MJ·m−2)47 ± 144 ± 242 ± 1
Residue (wt%)7.6 ± 0.39.8 ± 0.610.4 ± 0.6
* Phosphorus coating contents were calculated based on the phosphorus content value (7.89 wt%) of the TAEP monomer obtained by ICP-OES analysis.
Table 5. Elemental composition analysis performed on different areas (identified on Figure 11) of the cone calorimeter residues.
Table 5. Elemental composition analysis performed on different areas (identified on Figure 11) of the cone calorimeter residues.
Analysis AreaC
(wt%)
O (wt%)P
(wt%)
Ca
(wt%)
Mg
(wt%)
Mn
(wt%)
K
(wt%)
F0—Area 165.4527.330.314.411.080.980.44
F0—Area 212.2851.081.5921.954.844.853.40
F1—Area 381.6916.491.460.35---
F1—Area 481.1617.241.440.17---
F2—Area 576.4721.042.140.35---
F2—Area 680.7716.442.110.520.15--
Publisher’s Note: MDPI stays neutral with regard to jurisdictional claims in published maps and institutional affiliations.

Share and Cite

MDPI and ACS Style

Pellerin, S.; Samyn, F.; Duquesne, S.; Landry, V. Preparation and Characterisation of UV-Curable Flame Retardant Wood Coating Containing a Phosphorus Acrylate Monomer. Coatings 2022, 12, 1850. https://doi.org/10.3390/coatings12121850

AMA Style

Pellerin S, Samyn F, Duquesne S, Landry V. Preparation and Characterisation of UV-Curable Flame Retardant Wood Coating Containing a Phosphorus Acrylate Monomer. Coatings. 2022; 12(12):1850. https://doi.org/10.3390/coatings12121850

Chicago/Turabian Style

Pellerin, Solène, Fabienne Samyn, Sophie Duquesne, and Véronic Landry. 2022. "Preparation and Characterisation of UV-Curable Flame Retardant Wood Coating Containing a Phosphorus Acrylate Monomer" Coatings 12, no. 12: 1850. https://doi.org/10.3390/coatings12121850

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.

Article Metrics

Back to TopTop