Article

Preparation of Zn5Mo2O11·5H2O@Sulfonated Graphene by Template Method and Its Anticorrosion Mechanism in Polyurethane Coatings

College of Chemistry and Chemical Engineering, Shanghai University of Engineering Science, Shanghai 201620, China
*
Author to whom correspondence should be addressed.
Coatings 2022, 12(11), 1634; https://doi.org/10.3390/coatings12111634
Submission received: 22 September 2022 / Revised: 22 October 2022 / Accepted: 24 October 2022 / Published: 28 October 2022

Abstract

:
Currently, waterborne coatings are widely used, but their poor anticorrosion performance compared with solvent-based coatings hinders their further application. In this study, a series of Zn5Mo2O11·5H2O@sulfonated graphene (SZMO@SG) composites are prepared using the template method. SZMO@SG is a type of two-dimensional material with a large diameter and low thickness compared to traditional zinc molybdate. Combining SZMO@SG with waterborne hydroxy acrylic latex and isocyanate, the polyurethane coatings with 3 wt% SZMO@SG achieve the best anticorrosion performance in the 3.5 wt% NaCl immersion test. In electrochemical impedance spectroscopy (EIS), the charge transfer resistance (Rct) of polyurethane coatings with 3 wt% SZMO@SG reaches 283,100 Ω·cm2 after soaking in a 3.5 wt% NaCl solution for 48 h. Its corrosion potential and corrosion current are only −0.453 V and 1.71 × 10−3 mA/cm2, respectively. After metal substrate corrosion, the metal substrate of polyurethane coatings with SZMO@SG contain more Mo, Zn and low-state Fe atoms. It confirms that a passivation film was deposited on the metal substrate and prevents Fe from oxidation. The elemental content and distribution of the coatings after the NaCl solution immersion test indicate that SZMO@SG may have the Na+ adsorption function.

1. Introduction

Carbon steel is widely used in bridges, ships, pipelines, automobiles and other fields [1], but the economic loss caused by steel corrosion is inestimable [2]. Conversion coatings, especially phosphate conversion coatings, are widely applied to carbon steel, and improve its anticorrosion performance [3,4]. In order to broaden the application field of phosphate conversion coatings, researchers have explored various modification methods and deposition processes of conversion coatings [5,6]. For some waterborne anticorrosive coatings, their anticorrosive performance also depends on the phosphate deposition on the metal substrate [7].
Among the various resins available for organic coatings, polyurethane is a type of crosslinking curing resin [8,9], which is widely used and which dominates the coating industry. After adding a crosslinker such as isocyanate, a network structure can be formed, which improves its water resistance [10]. Waterborne polyurethane coatings, having the advantages of high gloss, high adhesion, and high hardness, are widely used in various fields [11,12,13]. Waterborne polyurethane coatings also have the advantages of low VOCs and environmental friendliness [14]. The size, shape, and chemical composition of the fillers are the important factors that affect the anticorrosion performance of coatings. The physical barrier performance of sheet fillers is significantly better than that of spherical fillers and linear fillers [15]. The reports also show that the chemical composition of the filler has a great impact on the self-healing and corrosion responses of the coatings [16,17].
Pollution problems have prompted scientists to look for novel environment-friendly corrosion inhibitors [18,19]. Molybdate, which has low toxicity in the environment compared to chromate, is better than phosphate in its anticorrosion performance [20,21,22]. It is expected to be an alternative high-performance anticorrosive filler. Early studies on molybdate mainly focused on passivation treatment on metal surfaces [23,24] to protect metal substrates, or on directly adding molybdate into coatings as functional fillers [25,26], so as to improve the anticorrosion performance of organic coatings. In recent years, many studies [27,28,29,30] have indicated that the performance of anticorrosion fillers can be further improved if multiple anticorrosion mechanisms are applied. Research on the new structures of molybdate fillers has emerged, such as ionic molybdate doping fillers [31] and molybdate intercalation modified hydrotalcite [32,33].
The template method is a very common way of synthesizing nano-materials such as nanoflakes, nanotubes, and nanoparticles [34]. It is easy to control the size and shape of nano-materials using the template method. Graphene is a type of two-dimensional sheet material with high conductivity and mechanical strength, which could be employed to modify the molybdate filler to improve its comprehensive performance. Sulfonic groups enhance the surface charge and chemical activity of the graphene [35]. Due to its sheet structure, graphene is often used as a template to prepare thin sheet materials [36,37]. Fillers with a sheet structure can form physical barriers, improving the anticorrosive performance of coatings.
In this study, the sheet molybdate anticorrosion filler with a high diameter-to-thickness ratio was synthesized. A novel sheet zinc molybdate composite filler (SZMO@SG) was prepared by depositing Zn(OH)2 on the surface of the sulfonated graphene and transforming to zinc molybdate. Sheet zinc molybdate can be obtained when the addition of sulfonated graphene reaches 1.5 wt%. Combining SZMO@SG with waterborne hydroxy acrylic latex and isocyanate, the polyurethane coatings with 3 wt% SZMO@SG achieve the best anticorrosion performance. After immersion in 3.5 wt% NaCl solution for 48 h, the Rct of polyurethane coatings with 3 wt% SZMO@SG reaches 283,100 Ω·cm2. Moreover, the anticorrosion mechanism of Zn5Mo2O11·5H2O was confirmed using EIS and an X-ray photoelectron spectrometer (XPS), which was lacking in in previous studies. SZMO@SG has several anticorrosion functions, including forming a physical barrier and a passivation film, and absorbing Na+. The sheet molybdate filler by template method can provide a long-term anticorrosion performance for waterborne polyurethane coatings.

2. Materials

2.1. Materials

The materials used in this study were shown below: zinc nitrate hexahydrate (Zn(NO3)2·6H2O, 99%, General-Reagent, Shanghai, China), ammonium molybdate ((NH4)6Mo7O24·4H2O, 99%, Sinopharm, Shanghai, China), ammonium hydroxide (NH3·H2O, 25%, Sinopharm, Shanghai, China), sodium dodecyl sulfate (SDS, 88%, Sinopharm, Shanghai, China), sulfonated graphene water dispersion (1%, Graphene-Tech Co., Ltd., Suzhou, China), waterborne hydroxy acrylic latex (Wanhua Chemical Group Co., Ltd., Yantai, China), isocyanate (Wanhua Chemical Group Co., Ltd., Yantai, China), and anhydrous ethanol (99.7%, General-Reagent, Shanghai, China). All the above reagents were used as received.

2.2. Synthesis of SZMO@SG Composite

SZMO@SG composites were prepared using the template method. The synthesis of Zn(OH)2@SG is referred to previous study [38]. Figure 1 is the schematic diagram of the preparation process of SZMO@SG. In the first step, a certain amount of SDS was added to 100 mL distilled water. A quantity of sulfonated graphene (SG) water dispersion was then added. The dispersion was treated by ultrasonication with 150 W power for 30 m, and then transferred into a 250 mL three-necked flask. A 25 mL 1.2 mol/L zinc nitrate solution (prepared with zinc nitrate hexahydrate) was added after 20 min, followed by 50 mL 1.25 mol/L ammonia solution (prepared with 25% ammonia) after 30 min. After reaction for 1 h, the solution was washed and filtered with distilled water three times.
In the second step, the product obtained in the previous step was placed in a 500 mL three-necked flask, and then 200 mL distilled water was added, followed by ultrasonication with 150 W power after 30 min. A 50 mL 0.087 mol/L ammonium molybdate solution (prepared with ammonium molybdate tetrahydrate) was added and reacted for 1 h under 80 °C with 500 rpm. Finally, the product was washed with distilled water and ethanol, and then dried in 50 °C.

2.3. Preparation of Polyurethane Coatings Based on SZMO@SG

The formula of coatings and dosage of composite fillers were based on our previous work [7]. An amount of SZMO@SG (weight ratio of 1 wt%, 3 wt%, or 5 wt%) was added to the waterborne hydroxy acrylic latex, and stirred for 30 m. A quantity of isocyanate was then added. Coatings were prepared on carbon steel for a water contact angle test, an electrochemical impedance spectroscopy test, and a 3.5 wt% NaCl solution immersion test. The film thickness was set as 50 ± 5 μm. Blank waterborne hydroxy acrylic latex was used as a control.

2.4. Characterization

The surface morphology, particle size, and lamellar thickness of Zn5Mo2O11·5H2O (ZMO) and SZMO@SG fillers were obtained using a scanning electron microscope (Zeiss Sigma 300, Zeiss, Oberkochen, Germany) at 3 kV. X-ray diffraction (XRD, PANalytical, Almelo, Netherlands) patterns of SG, ZMO, and SZMO@SG were recorded using an X’Pert PRO MPD and CuKα as the radiation source (λ = 0.15406 nm). A Fourier transform infrared spectrometer (Nicolet, Thermo Fisher Scientific, Massachusetts, America) was used to obtain the functional group information of the SG, ZMO, and SZMO@SG. The surface elements of SG, ZMO, and SZMO@SG were tested using an X-ray photoelectron spectrometer (Axis Ultra DLD Kratos Axis SUPRA, KRATOS, Manchester, Britain) with monochromatic AlKα sources. The C 1s signal was calibrated to 284.8 eV. The peak fitting method depends on the atomic spin splitting. The single peak fitting was applied to C 1s and O 1s. The double peaks fitting was applied to Zn 2p, Fe 2p, S 2p, and Mo 3d. Before the electrochemical test, the carbon steel coated with coatings was cut, and the edge and back surface of the sample was sealed with a mixture of rosin: paraffin = 1:1. The coatings with a retention area of 1 cm × 1 cm were tested using the electrochemical method. After soaking in 3.5 wt% NaCl solution for a period of time, the EIS and Tafel curves of coatings were obtained using an electrochemical workstation CHI660E (Shanghai Chenhua Device Co., Shanghai, China). Both Tafel curves and EIS testing were carried out with respect to SCE. Before the water contact angle test, coated carbon steel was soaked in deionized water for a certain period of time, then dried at room temperature for 5 min. A water contact angle tester (Shanghai Pushen Testing instrument Co., Ltd., Shanghai, China) was used to obtain the contact angle data of coatings.

3. Results and Discussion

3.1. Characterization of SZMO@SG

The FT-IR spectra of SG, ZMO, and SZMO@SG was shown in Figure 2. In the FT-IR spectra of SG, the infrared absorption at 1705 cm−1, 1615 cm−1, 1141 cm−1, and 1033 cm−1 corresponds to the stretching vibration absorption of C=O, C=C, O=S=O, and C–O [7,39], respectively. The wide peak in the range of 3300~3450 cm−1 is the stretching vibration absorption of sulfonated graphene with –OH [40]. The stretching vibration and bending vibration of molybdate ion corresponding to 800~930 cm−1 are shown in the spectrum of ZMO [41,42]. The wide peak in 3200~3250 cm−1 proves that ZMO has crystal water [43]. In addition, the absorption peak of 1610 cm−1 is also related to the bending vibration of crystal water [44]. The absorption peak at 480 cm−1 is ascribed to the Zn–O. In the spectrum of SZMO@SG, the absorption peaks of C=O, O=S=O, and C–O of sulfonated graphene are located at 1725 cm−1, 1143~1233 cm−1, and 1030 cm−1, respectively. It can be concluded that the prepared composite filler was a compound of ZMO and sulfonated graphene.
To discuss the surface chemical composition of SG, ZMO, and SZMO@SG, the elemental composition and surface elemental valence states of SG, ZMO, and SZMO@SG are characterized by XPS, and the results are shown in Figure 3. In the spectrum of SG C 1s, the three peaks at 284.8 eV, 286.2 eV, and 288.8 eV are attributed to C–C, C–O, and C=O in the sulfonated graphene [45]. In the O 1s spectrum, the peaks at 532.7 eV, 533.5 eV, and 532.0 eV are ascribed to O=S=O, C–O, and carboxyl –OH, respectively [46]. The peaks of 164.3 eV and 169.3 eV in S 2p correspond to C–S and S–O, which proves the existence of sulfonic acid groups in the graphene surface. In the O 1s spectrum of ZMO, the 530.5 eV and 532.1 eV peaks are attributed to molybdate and binding water [47], and the 531.2 eV peak is considered to be the surface hydroxyls. There are two strong peaks of 1021.5 eV and 1044.5 eV in the spectrum of Zn 2p, which are related to the binding energies of Zn 2p3/2 and Zn 2p1/2, respectively. The difference between the two peaks’ binding energies δ is 23.0 eV. It can be inferred from the value of δ that Zn element exists in a bivalent state in ZMO [48]. In the Mo 3d spectrum, both 232.7 eV and 235.8 eV are characteristic peaks of Mo6+, which are associated with the binding energies of Mo 3d5/2 and Mo 3d1/2 [49].
The XPS spectrum of SZMO@SG illustrates that O 1s has three peak values of 530.6 eV, 531.3 eV, and 532.3 eV, which are consistent with molybdate, surface hydroxyls, and binding water. The binding energies of Zn 2p3/2 and Zn 2p1/2 of Zn 2p are located at 1021.7 eV and 1044.7 eV. Compared with ZMO, Mo 3d of SZMO@SG only has Mo 3d5/2 and Mo 3d3/2 signals at 232.7 eV and 235.9 eV. The C1s spectra of SZMO@SG have C–C, C–O–C, and C=O peaks of SG at 284.8 eV, 286.3 eV, and 288.8 eV. On the other hand, in the S 2p spectrum of SZMO@SG, the signal is weak at the positions of 162.9 eV and 169.0 eV. This is because the sampling depth of XPS is only 2~5 nm, while the outer layer of SZMO@SG is mostly composed of molybdate with less S element content on the surface. The XPS analysis reflects the fact that ZMO and SZMO@SG have similar atomic ratios of Zn:Mo, which are 1.78:1 and 1.74:1, respectively. We were able to confirm from the XPS spectra that the samples prepared are composites of ZMO encapsulated SG.
XRD can be used to further study the crystal structure of the fillers. As shown in Figure 4, strong characteristic peaks appear at 11.7° and 20.7° in the XRD patterns of the SG. The peak of 11.7° is commonly regarded as the layer spacing of graphene materials. According to the Bragg equation, the layer spacing of sulfonated graphene can be calculated as 0.76 nm, which is close to the data in the literature [50]. The 20.7° peak corresponds to the 0.43 nm layer spacing of graphite, indicating that the sulfonated graphene used has an incomplete oxidation structure [51]. There are three characteristic peaks of 12.3°, 26.6°, and 34.0° in the XRD pattern of ZMO, which correspond to the crystal faces of (003), (015), and (021), respectively. The lattice constants a = 6.1423 Å, b = 6.1423 Å, and c = 21.6347 Å were calculated from the data of the XRD patterns, which were very similar to JCPDS No. 30-1486 Zn5Mo2O11·5H2O (a = 6.136 Å, b = 6.136 Å, and c = 21.6 Å) [52]. The XRD patterns of SZMO@SG show a great similarity with Zn5Mo2O11·5H2O, and the signals at 12.1°, 26.5°, and 34.0° correspond to the crystal planes of (003), (015), and (021). The calculated lattice constants are a = 6.1271 Å, b = 6.1271 Å, and c = 21.5753 Å. The disappearance of SG characteristic peaks in the XRD patterns of SZMO@SG indicates that the lamellar layers of SG are filled with deposited Zn5Mo2O11·5H2O, and the spacing between SG layers of SZMO@SG is much larger than that of pure SG. The weak peaks at 2 θ = 20.2°, 20.9°, 27.2°, and 27.8° correspond to (011), (101), (111), and (102) crystal planes, indicating that the filler contains a small amount of Zn(OH)2. However, the Zn5Mo2O11·5H2O dominates in the composite filler. The XRD spectra proved that the main components of ZMO and SZMO@SG are Zn5Mo2O11·5H2O, and also indirectly proved that SZMO@SG is a composite filler from ZMO and SG.
SEM images of ZMO and SZMO@SG are shown in Figure 5. It shows that the particle size of ZMO is in the range of 15~40 μm in Figure 5a. In the ZMO crystal growth process, the small irregular ZMO particles are generated first, and then the small ZMO particles are assembled to form large ZMO particles with rough surfaces. Therefore, the grooves formed by the splicing of the particles can be clearly seen on the ZMO surface. In addition, due to the hexagonal structure of Zn5Mo2O11·5H2O, ZMO has numerous ~100 nm sheet folded structures. SEM images of SZMO@SG with moderate SG are shown in Figure 5b, which show a disk-like morphology. The diameter of SZMO@SG is ~30 μm, and the thickness of the lamellar is ~100 nm. Due to the existence of the template, small SZMO@SG particles were formed in the growth process. However, the concentration of SZMO@SG particles is appropriate to stack in parallel and grow radially. Finally, large SZMO@SG particles are formed. The grooves formed by splicing can still be seen in Figure 5b, but there is almost no sheet folded structure compared with that in Figure 5a. As can be seen in Figure 5c, after the addition of 0.6 wt% SG, the size of SZMO@SG particles prepared was in the range of 1~10 μm, and the thickness of the lamella was ~200 nm. When the amount of SG exceeded a certain amount, the size of initially formed SZMO@SG particles was smaller, and the number of particles per unit volume of solution increased sharply. The different size and orientation of SZMO@SG particles can be spliced in different directions, and, finally, SZMO@SG particles with smooth surface but folded structure were synthesized.

3.2. Corrosion Resistance of Coatings with SZMO@SG

The change in the coating contact angle with the soaking time reflects the transformation of hydrophilic or hydrophobic property of the surface of the coatings. The curves of the contact angles of the coatings are shown in Figure 6.
It can be seen that the contact angle of the coatings tends to decrease with the increase in immersion time. During immersion, water molecules were absorbed on the surface of the coatings, which led to the permeation of the corrosive medium on the surface of the coatings more easily. Moreover, the coating was constantly damaged in the corrosion process, and the increasing of defects and cracks on the surface of the coating reduces the contact angle and anticorrosion performance. The contact angle of the control and the sample with 1 wt% SZMO@SG decreased the most, while the contact angle of samples with 3 wt% and 5 wt% fillers did not change significantly. Therefore, high-content SZMO@SG coatings (3 wt% and 5 wt%) may be beneficial for improving the anticorrosion performance.
The variation of element distribution in the cross-section of the coatings with high magnification is shown in Figure 7 and the corresponding data is shown in Table 1. It can be clearly seen that the signals of the Na and Cl element for the control were enhanced and uniformly distributed in the coatings after immersion. The proportion of Na was higher than that of Cl, proving that the permeation rate of Na+ in the coatings is faster than that of Cl during immersion. As can be seen from Figure 7c,d, Zn and Mo signals appeared in the coatings after the addition of SZMO@SG, and Zn and Mo even overlapped with some O signals. After soaking in NaCl solution, Na signals were still enhanced. In addition, the distribution of Na overlapped with Zn and Mo, which may be due to the adsorption and enrichment of Na+ on SZMO@SG surface.
In order to visually measure the corrosion resistance of coatings with different SZMO@SG content, the samples were immersed in 3.5 wt% NaCl for a test. As shown in Figure 8a, it was found that the corrosion resistance of the coatings increased first, and then decreased with the increase in the amount of SZMO@SG. The control without the addition of SZMO@SG filler showed serious corrosion after soaking for 96 h. The corrosion medium penetrated completely into the coatings, and diffused into the interface between the carbon steel and coatings. The control also developed blistering above the soaking line after soaking for 288 h. When the addition of SZMO@SG reached 1 wt%, the coatings showed serious corrosion at the soaking line between 288 h and 480 h, and there were also traces of penetration by the corrosion medium above the soaking line. When the amount of SZMO@SG increased to 3 wt%, the polyurethane coatings only showed slight corrosion at 1 cm near the immersion line after immersing for 1008 h. There was only one rust spot below the immersion line, almost no corrosion trace on the other position of sample, and no obvious traces of penetration by the corrosion medium above the immersion line was observed. However, when the amount of SZMO@SG reached a high level of 5 wt%, the corrosion resistance of the coatings decreased and a large number of rust spots appeared after 480 h immersion. The results indicate that adding 3 wt% SZMO@SG fillers can effectively prevent the penetration of corrosion medium in the coatings, improve the corrosion resistance of the coatings, and effectively protect the metal substrate.
Moreover, rusty spots appeared on the surface of coatings with 3 wt% ZMO after soaking in a 3.5 wt% NaCl solution for 288 h. The corrosion resistance of 3 wt% ZMO coatings is obviously weaker than 3 wt% SZMO@SG coatings. Because the ZMO could not form the layer-by-layer structure in the coatings. In addition, due to the poor compatibility between resin and inorganic fillers, ZMO coatings have more defects compared to the SZMO@SG coatings, leading to the formation of corrosive medium permeation channels in the coatings. Therefore, the corrosive medium is more likely to penetrate into the 3 wt% ZMO coatings during immersion.
After soaking for 1008 h in a 3.5 wt% NaCl solution, the control and coatings with 3 wt% SZMO@SG were peeled by soaking in acetone for 24 h. To investigate the chemical changes of coated metal substrates after immersion, a XPS test was carried out on the surface of metal substrate. The change in Fe valence state after corrosion can be determined by Fe 2p spectrum, as shown in Figure 8, where 724.8 eV, 719.4 eV, and 711.6 eV are characteristic peaks of Fe3+ [53,54], and the characteristic peaks of 715.7 eV and 710.0 eV are attributed to Fe2+ [55,56]. Using software to calculate the peak area, the atomic ratio of the two valence states of Fe3+:Fe2+ is 1.56:1, which is close to the Fe content in Fe3O4. The element valence states on the surface of metal substrate of coatings with 3 wt% SZMO are shown in Figure 8c–e. Due to the deposition of a passivation film on the metal substrate, Zn and Mo signals became stronger, and Fe signal became weaker. The Fe 2p spectrum can further verify the anticorrosion mechanism of SZMO@SG. The characteristic peaks of Fe2+ are ascribed to 708.3 eV, 709.8 eV, 711.1 eV, 712.4 eV, and 715.7 eV, while the weak characteristic peak of Fe3+ is located at 711.1 eV. In addition, there is also a weak characteristic peak of 0 valence state Fe at 705.9 eV. The ratio of Fe3+:Fe2+ was calculated as 1:10.08, indicating that the passivation film effectively prevents the oxidation of Fe. In Mo 3d and Zn 2p spectra, Zn2+ and molybdate ions were also deposited on the carbon steel, and these ions were involved in the formation of a passivation layer. Compared with the Fe 2p spectrum of the control in Figure 8a, the carbon steel coated with coatings of 3 wt% SZMO@SG contained more Fe2+ on its surface after corrosion, and there was even 0 valence Fe on the surface, which proves that the passivation layer formed in the corrosion of the coatings containing SZMO@SG can effectively prevent the oxidation of Fe. Element and valence state analysis indicate that the passivation layer is mainly composed of metal hydroxide and iron molybdate.
The potential dynamic polarization curve is often used to characterize the anticorrosive performance of the coatings [57,58]. The coated carbon steel was soaked in 3.5 wt% NaCl solution for different times for testing. Ecorr, icorr, ba, and bc are the corrosion potential, corrosion current, anode slope, and cathode slope in sequence. The protection efficiency (η) can be calculated by Equation (1) [57]:
η ( % ) = 100 % × ( 1 ( i c o r r , i i c o r r , b ) )
where icorr,i and icorr,b are the corrosion current of coatings with SZMO@SG and controls, respectively.
As shown in Figure 9 and Table 2, the addition of SZMO@SG had a significant effect on the potentiodynamic polarization curves and corrosion current of the coatings. As the addition of SZMO@SG increased, the corrosion potential increased from −0.586 V for control to −0.453 V for coatings with a 3 wt% composite filler. The corrosion current decreased with the increase in SZMO@SG. When the addition of SZMO@SG was 3 wt%, the 48 h corrosion current reached the lowest value of 1.71 × 10−3 mA/cm2, while the corrosion current of control reached 6.71 × 10−3 mA/cm2. The unique lamellar structure of SZMO@SG obstructed the channels of corrosive medium in coatings, blocking the penetration of H2O, O2, and ions. Moreover, the molybdate ions reacted with Fe3+ and Fe2+, forming iron molybdate passivation films on carbon steel [49,59], which effectively reduced the corrosion current. The change in corrosion potential of the SZMO@SG coatings from 48 h to 840 h may reflect the transformation of the corrosion mechanism from mainly anode passivation to both cathode and anode passivation. The metal substrate of coatings with 3 wt% SZMO@SG was confirmed to have metal hydroxide deposited on it, based on the XPS (Figure 8). Moreover, the cathodic part of Tafel curve moved towards negative potential, which indicates that the hydroxide deposited on the metal substrate cathode could hinder the corrosion reaction of cathode. In addition, coatings with 5 wt% SZMO@SG have the larger Icorr value than that of 3 wt%, indicating that the increase in coating defects and ion channels reduces the anticorrosion performance of coatings.
EIS is a common method for evaluating the corrosion resistance of coatings. Previous studies [60,61] reported that the size of capacitive arc reactance has a great correlation with the anticorrosion performance of coatings. As shown in Figure 10, it can be seen that the capacitance arc radius increases with the increase in SZMO@SG, and reaches its highest value when the addition of SZMO@SG reaches 3 wt%. However, too much SZMO@SG will increase the coating defects and reduce the anticorrosion performance of coatings. The EIS results are consistent with the results of the 3.5 wt% NaCl immersion test. It is easy to confirm that the protective effect of the coatings and the capacitance arc radius constantly decreases with the increase in soaking time, but coatings with 3 wt% SZMO@SG have the largest capacitance arc radius.
As shown in the Bode phase angle diagram (Figure 11), all the coatings have incomplete time constants in the high frequency region and complete time constants in the mid- and low-frequency region after immersion. This is because the corrosive medium has reached the metal substrate. According to Figure 12, in the Bode plots of 48 h and 144 h, the 3 wt% SZMO@SG coating always has the largest impedance modulus in the high-frequency region. It is attributed to the physical barrier of SZMO@SG. However, in the bode plots of 840 h, the impedance modulus of 3 wt% SZMO@SG coatings decreases significantly due to the penetration of electrolyte. In the low-frequency region, the coatings with 3 wt% SZMO@SG have the highest impedance |Z| of more than 105 Ω (48 h), and it still reached more than 6000 Ω after being immersed in a 3.5 wt% NaCl solution for 840 h.
In order to further study the anticorrosion mechanism of coatings, an equivalent circuit diagram (Figure 13) was obtained by fitting the data in Figure 10. The fitting parameters are shown in Table 3. In the equivalent circuit, Rs, Rf, and Rct are solution resistance, film resistance, and charge transfer resistance, respectively. CPEf and CPEdl represent film capacitance and double layer capacitance, respectively. After soaking for 48 h, it can be seen that the Rf values of the SZMO@SG coatings are generally higher than the control, because the flake structure can form better physical barrier effect and prevent the penetration of corrosion medium. However, the Rf of 5 wt% SZMO@SG coatings is significantly lower than 3 wt% SZMO@SG coatings. It can be confirmed that there were more corrosion medium channels in the 5 wt% SZMO@SG coatings. The defects inside the 5 wt% SZMO@SG coatings led to the generation of corrosion medium channels. To further study the porosity of coatings, Equation (2) was used to calculate the porosity of coatings [62,63].
P = R p s R p 10 Δ E c o r r   b a
In the equation, P is porosity, Rps is the polarization resistance of the substrate, Rp is the polarization resistance of the samples, ΔEcorr is the potential difference between the uncoated and the coated substrate, ba is the anodic Tafel coefficient of the substrate. The electrochemical parameter of carbon steel can be obtained from the related reference [64,65]. In Table 3, the 3 wt% SZMO@SG coatings have the lowest porosity. After immersion for 840 h, the porosities of the control and the 5 wt% SZMO@SG coatings had significantly increased. However, the porosity of 3 wt% coating was only 0.32%. It can be confirmed that the size and number of pores increased inside the control and 5 wt% coatings. It also can be proved that SZMO@SG can form a physical barrier inside the coatings.
CPEf is related to electrolyte penetration in the coatings. The lowest CPEf further indicates minimal penetration of the corrosive medium into the 3 wt% SZMO@SG coatings. In Table 3, Rct of coatings with SZMO@SG increased significantly. After soaking for 48 h, with the increase in SZMO@SG content, Rct increased from 8608 Ω·cm2 (control) to 283,100 Ω·cm2 (3 wt% fillers), and then decreased. This proves that the passivation layer is generated at the interface between the coatings and the substrate, which can block ion and charge transfer. The formation of a passivation film is attributed to the reaction of molybdate with Fe2+ and Fe3+, forming FeMoO4 and Fe2(MoO4)3. Rct of 3 wt% and 5 wt% SZMO@SG coatings increased significantly compared to other coatings, proving the high reaction activity of Fe ion and molybdate. The passivation film was stable and insoluble; even after being immersed for 840 h, Rct of 3 wt% SZMO@SG coatings still reached 51,910 Ω·cm2. It can be proved that the passivation film plays a dominant role in late corrosion resistance. Due to the corrosion medium channels inside 5 wt% SZMO@SG coatings, most of the molybdate was released into the external solution, leading to a slight reaction between the molybdate and Fe ions. Therefore, Rct of the 5 wt% SZMO@SG coating was much smaller than the 3 wt% SZMO@SG coating.

3.3. Anticorrosion Mechanism of Polyurethane Coatings with SZMO@SG

From the above discussion it can be concluded that the appropriate dosage of SZMO@SG can effectively improve the corrosion resistance of polyurethane coatings. The anticorrosion mechanism of SZMO@SG coatings was shown in Figure 14. At the initial stage of immersion, the lamellar structure of SZMO@SG forms a physical barrier in the coatings, which can effectively prevent the infiltration of corrosion medium. In the middle and late stages of soaking, MoO42− and Zn2+ generated by SZMO@SG dissolution can capture Fe2+, Fe3+, and OH, forming passivation layer. The passivation layer can also prevent carbon steel from contact with the corrosion medium. The reaction for the forming of the passivation layer is as follows [43]:
2Fe3+ + 3 MoO42− + n H2O → Fe2(MoO4)3·n H2O
Fe2+ + MoO42− + n H2O → FeMoO4·n H2O
Zn2+ + 2 OH → Zn(OH)2
Zn(OH)2 generated by the hydrolysis of SZMO@SG can adsorb Na+ and Cl [32,41], which can further improve the anticorrosion performance of the coatings, confirmed in Figure 7. Therefore, SZMO@SG has three anticorrosive functions: forming physical barrier, passivating the metal substrate, and absorbing Na+ and Cl. In contrast to traditional anticorrosive fillers, SZMO@SG can significantly improve the anticorrosive performance of waterborne polyurethane coatings.

4. Conclusions

In this study, SZMO@SG was successfully prepared and mixed with hydroxy acrylate latex, significantly improving the anticorrosive performance of waterborne polyurethane coatings. The SZMO@SG fillers have a lamellar structure with the optimized SG addition of 1.5 wt%. The optimized corrosion resistance of coatings was obtained when the dosage of SZMO@SG is 3 wt%, but higher filler addition will diminish the anticorrosion performance of coatings. For the optimized coatings with 3 wt% SZMO@SG, the corrosion current density has the lowest value of 1.71 × 10−3 mA/cm2, and the maximum charge transfer resistance of the coatings reaches 283,100 Ω·cm2. Even after soaking in a 3.5 wt% NaCl solution for 840 h, its Rct still reached 51,910 Ω·cm2. Through the EIS and metal substrate XPS, it can be confirmed that the passivation film was deposited on the interface between coatings and metal substrate. The passivation film blocks the ion and charge transfer, and prevents Fe from oxidation. Furthermore, the cross-section of the coatings EDS confirms the Na+ adsorption of SZMO@SG. SZMO@SG is a novel anticorrosion filler with several anticorrosion functions, which could be further applied in other waterborne organic coatings.

Author Contributions

Conceptualization, Z.Z. and S.W. (Shaoguo Wen); methodology, Z.Z.; visualization, Z.Z.; validation, J.X.; formal analysis, W.L. and J.S.; data curation, S.W. (Song Wang), W.L. and J.S.; writing-original draft preparation, Z.Z.; writing-review and editing, Z.Z., K.C. and J.W.; supervision, S.W. (Shaoguo Wen); project administration, S.W. (Shaoguo Wen). All authors have read and agreed to the published version of the manuscript.

Funding

This research received no external funding.

Institutional Review Board Statement

Not applicable.

Informed Consent Statement

Not applicable.

Data Availability Statement

The data presented in this study are available in the article.

Conflicts of Interest

The authors declare no conflict of interest.

References

  1. Trivedi, P.A.; Solanki, N.M.; Butani, N.; Parikh, P.A. Investigation on corrosion control of mild steel buried in soil by spent FCC catalyst coating. J. Ind. Eng. Chem. 2014, 20, 2264–2271. [Google Scholar] [CrossRef]
  2. Xu, B.; Liu, Y.; Yin, X.; Yang, W.; Chen, Y. Experimental and theoretical study of corrosion inhibition of 3-pyridinecarbozalde thiosemicarbazone for mild steel in hydrochloric acid. Corros. Sci. 2013, 74, 206–213. [Google Scholar] [CrossRef]
  3. Jegannathan, S.; Sankara Narayanan, T.S.N.; Ravichandran, K.; Rajeswari, S. Performance of zinc phosphate coatings obtained by cathodic electrochemical treatment in accelerated corrosion tests. Electrochim. Acta 2005, 51, 247–256. [Google Scholar] [CrossRef]
  4. De Freitas Cunha Lins, V.; de Andrade Reis, G.F.; de Araujo, C.R.; Matencio, T. Electrochemical impedance spectroscopy and linear polarization applied to evaluation of porosity of phosphate conversion coatings on electrogalvanized steels. Appl. Surf. Sci. 2006, 253, 2875–2884. [Google Scholar] [CrossRef]
  5. Kathavate, V.S.; Pawar, D.N.; Bagal, N.S.; Deshpande, P.P. Electrodeposition and characterization of nano ZnO incorporated phosphate coatings for the corrosion protection performance of low carbon steel. J. Alloys Compd. 2020, 823, 153812. [Google Scholar] [CrossRef]
  6. Kathavate, V.S.; Deshpande, P.P. Role of nano TiO2 and nano ZnO particles on enhancing the electrochemical and mechanical properties of electrochemically deposited phosphate coatings. Surf. Coat. Technol. 2020, 394, 125902. [Google Scholar] [CrossRef]
  7. Wu, Y.; Wen, S.; Chen, K.; Wang, J.; Wang, G.; Sun, K. Enhanced corrosion resistance of waterborne polyurethane containing sulfonated graphene/zinc phosphate composites. Prog. Org. Coat. 2019, 132, 409–416. [Google Scholar] [CrossRef]
  8. Gite, V.V.; Mahulikar, P.P.; Hundiwale, D.G. Preparation and properties of polyurethane coatings based on acrylic polyols and trimer of isophorone diisocyanate. Prog. Org. Coat. 2010, 68, 307–312. [Google Scholar] [CrossRef]
  9. Córdoba, C.A.; Collins, S.E.; Passeggi, M.C.G.; Vaillard, S.E.; Gugliotta, L.M.; Minari, R.J. Crosslinkable acrylic-melamine latex produced by miniemulsion polymerization. Prog. Org. Coat. 2018, 118, 82–90. [Google Scholar] [CrossRef]
  10. Li, J.; Ecco, L.; Delmas, G.; Whitehouse, N.; Collins, P.; Deflorian, F.; Pan, J. In-Situ AFM and EIS Study of Waterborne Acrylic Latex Coatings for Corrosion Protection of Carbon Steel. J. Electrochem. Soc. 2015, 162, 55–63. [Google Scholar] [CrossRef]
  11. Nguyen, T.V.; Le, X.H.; Dao, P.H.; Decker, C.; Nguyen-Tri, P. Stability of acrylic polyurethane coatings under accelerated aging tests and natural outdoor exposure: The critical role of the used photo-stabilizers. Prog. Org. Coat. 2018, 124, 137–146. [Google Scholar] [CrossRef]
  12. Nguyen, T.N.L.; Do, T.V.; Nguyen, T.V.; Dao, P.H.; Trinh, V.T.; Mac, V.P.; Nguyen, A.H.; Dinh, D.A.; Nguyen, T.A.; Vo, T.K.A.; et al. Antimicrobial activity of acrylic polyurethane/Fe3O4-Ag nanocomposite coating. Prog. Org. Coat. 2019, 132, 15–20. [Google Scholar] [CrossRef]
  13. Ma, G.; Guan, T.; Hou, C.; Wu, J.; Wang, G.; Ji, X.; Wang, B. Preparation, properties and application of waterborne hydroxyl-functional polyurethane/acrylic emulsions in two-component coatings. J. Coat. Technol. Res. 2015, 12, 505–512. [Google Scholar] [CrossRef]
  14. Barbosa, J.V.; Veludo, E.; Moniz, J.; Mendes, A.; Magalhães, F.D.; Bastos, M.M.S.M. Low VOC self-crosslinking waterborne acrylic coatings incorporating fatty acid derivatives. Prog. Org. Coat. 2013, 76, 1691–1696. [Google Scholar] [CrossRef]
  15. Li, Z.; Li, J.; Cui, J.; Qiu, H.; Yang, G.; Zheng, S.; Yang, J. Dispersion and parallel assembly of sulfonated graphene in waterborne epoxy anticorrosion coatings. J. Mater. Chem. A 2019, 7, 17937–17946. [Google Scholar] [CrossRef]
  16. Mersagh Dezfuli, S.; Sabzi, M. Deposition of self-healing thin films by the sol–gel method: A review of layer-deposition mechanisms and activation of self-healing mechanisms. Appl. Phys. A-Mater. 2019, 125, 557. [Google Scholar] [CrossRef]
  17. Sabzi, M.; Far, S.M.; Dezfuli, S.M. Characterization of bioactivity behavior and corrosion responses of hydroxyapatite-ZnO nanostructured coating deposited on NiTi shape memory alloy. Ceram. Int. 2018, 44, 21395–21405. [Google Scholar] [CrossRef]
  18. Fernine, Y.; Salim, R.; Arrousse, N.; Haldhar, R.; El Hajjaji, F.; Kim, S.C.; Touhami, M.E.; Taleb, M. Anti-corrosion performance of Ocimum basilicum seed extract as environmental friendly inhibitors for mild steel in HCl solution: Evaluations of electrochemical, EDX, DFT and Monte Carlo. J. Mol. Liq. 2022, 355, 118867. [Google Scholar] [CrossRef]
  19. Haldhar, R.; Asrafali, S.P.; Raorane, C.J.; Periyasamy, T.; Kim, S.C. Performance of cross-linked polymers as a potential anticorrosive coating for low carbon steel in acidic condition: Experimental and computational studies. J. Mol. Liq. 2022, 360, 119384. [Google Scholar] [CrossRef]
  20. Liu, D.; Yang, Z.; Wang, Z.; Zhang, C. Synthesis and evaluation of corrosion resistance of molybdate-based conversion coatings on electroplated zinc. Surf. Coat. Technol. 2010, 205, 2328–2334. [Google Scholar] [CrossRef]
  21. Shahini, M.H.; Mohammadloo, H.E.; Ramezanzadeh, B. Recent advances in steel surface treatment via novel/green conversion coatings for anti-corrosion applications: A review study. J. Coat. Technol. Res. 2022, 19, 159–199. [Google Scholar] [CrossRef]
  22. Mohammadloo, H.E.; Sarabi, A.A. Titanium composite conversion coating formation on CRS In the presence of Mo and Ni ions: Electrochemical and microstructure characterizations. Appl. Surf. Sci. 2016, 387, 252–259. [Google Scholar] [CrossRef]
  23. Tsai, C.; Liu, J.; Chen, P.; Lin, C. A two-step roll coating phosphate/molybdate passivation treatment for hot-dip galvanized steel sheet. Corros. Sci. 2010, 52, 3385–3393. [Google Scholar] [CrossRef]
  24. Yao, Y.; Zhou, Y.; Zhao, C.; Han, Y.; Zhao, C. Preparation and Corrosion Resistance Property of Molybdate Conversion Coatings Containing SiO2 Nanoparticles. J. Electrochem. Soc. 2013, 160, 185–188. [Google Scholar] [CrossRef]
  25. Eduok, U.; Szpunar, J. Ultrasound-assisted synthesis of zinc molybdate nanocrystals and molybdate-doped epoxy/PDMS nanocomposite coatings for Mg alloy Protection. Ultrason. Sonochem. 2018, 44, 288–298. [Google Scholar] [CrossRef]
  26. Kapole, S.A.; Bhanvase, B.A.; Pinjari, D.V.; Gogate, P.R.; Kulkarni, R.D.; Sonawane, S.H.; Pandit, A.B. Investigation of corrosion inhibition performance of ultrasonically prepared sodium zinc molybdate nanopigment in two-pack epoxy-polyamide coating. Compos. Interfaces 2014, 21, 833–852. [Google Scholar] [CrossRef]
  27. Tedim, J.; Poznyak, S.K.; Kuznetsova, A.; Raps, D.; Hack, T.; Zheludkevich, M.L.; Ferreira, M.G.S. Enhancement of Active Corrosion Protection via Combination of Inhibitor-Loaded Nanocontainers. ACS Appl. Mater. Interfaces 2010, 2, 1528–1535. [Google Scholar] [CrossRef]
  28. Liu, A.; Tian, H.; Li, W.; Wang, W.; Gao, X.; Han, P.; Ding, R. Delamination and self-assembly of layered double hydroxides for enhanced loading capacity and corrosion protection performance. Appl. Surf. Sci. 2018, 462, 175–186. [Google Scholar] [CrossRef]
  29. Trung, V.Q.; Hoan, P.V.; Phung, D.Q.; Duc, L.M.; Hang, L.T.T. Double corrosion protection mechanism of molybdate-doped polypyrrole/montmorillonite nanocompos ites. J. Exp. Nanosci. 2014, 9, 282–292. [Google Scholar] [CrossRef] [Green Version]
  30. Alexander, L.; Otto, V.D.B.; Jan, W.; Iris, D.G.; Herman, T. A Multiple-Action Self-Healing Coating. Front. Mater. 2016, 2, 73. [Google Scholar]
  31. Chen, Z.; Yang, W.; Yin, X.; Chen, Y.; Liu, Y.; Xu, B. Corrosion protection of 304 stainless steel from a smart conducting polypyrrole coating doped with pH-sensitive molybdate-loaded TiO2 nanocontainers. Prog. Org. Coat. 2020, 146, 105750. [Google Scholar] [CrossRef]
  32. Leal, D.A.; Wypych, F.; Marino, C.E.B. Zinc-Layered Hydroxide Salt Intercalated with Molybdate Anions as a New Smart Nanocontainer for Active Corrosion Protection of Carbon Steel. ACS Appl. Mater. Interfaces 2020, 12, 19823–19833. [Google Scholar] [CrossRef] [PubMed]
  33. Olya, N.; Ghasemi, E.; Ramezanzadeh, B.; Mahdavian, M. Synthesis, characterizatio n and protective functioning of surface decorated Zn-Al layered double hydroxide with SiO2 nano-particles. Surf. Coat. Technol. 2020, 387, 125512. [Google Scholar] [CrossRef]
  34. Pérez-Page, M.; Yu, E.; Li, J.; Rahman, M.; Dryden, D.M.; Vidu, R.; Stroeve, P. Template-based syntheses for shape controlled nanostructures. Adv. Colloid Interface Sci. 2016, 234, 51–79. [Google Scholar] [CrossRef] [PubMed] [Green Version]
  35. Oger, N.; Lin, Y.F.; Labrugère, C.; Grognec, E.L.; Rataboul, F.; Felpin, F. Practical and scalable synthesis of sulfonated graphene. Carbon 2016, 96, 342–350. [Google Scholar] [CrossRef]
  36. Li, Z.; Wu, S.; Lv, W.; Shao, J.; Kang, F.; Yang, Q. Graphene Emerges as a Versatile Template for Materials Preparation. Small 2016, 12, 2674–2688. [Google Scholar] [CrossRef] [PubMed]
  37. Wang, P.; He, F.; Wang, J.; Yu, H.; Zhao, L. Graphene oxide nanosheets as an effective template for the synthesis of porous TiO2 film in dye-sensitized solar cells. Appl. Surf. Sci. 2015, 358, 175–180. [Google Scholar] [CrossRef]
  38. Yu, D.; Wen, S.; Yang, J.; Wang, J.; Chen, Y.; Luo, J.; Wu, Y. RGO modified ZnAl-LDH as epoxy nanostructure filler: A novel synthetic approach to anticorrosive waterborne coating. Surf. Coat. Technol. 2017, 326, 207–215. [Google Scholar] [CrossRef]
  39. Ma, J.; Li, W.; Guan, S.; Liu, Q.; Li, Q.; Zhu, C.; Yang, T.; Ogunbiyia, A.T.; Ma, L. Efficient catalytic conversion of corn stalk and xylose into furfural over sulfonated graphene in γ-valerolactone. RSC Adv. 2019, 9, 10569–10577. [Google Scholar] [CrossRef] [PubMed] [Green Version]
  40. Naeimi, H.; Golestanzadeh, M. Highly sulfonated graphene and graphene oxide nanosheets as heterogeneous nanocatalysts in green synthesis of bisphenolic antioxidants under solvent free conditions. RSC Adv. 2014, 4, 56475–56488. [Google Scholar] [CrossRef]
  41. Singh, H.K.; Yeole, K.V.; Mhaske, S.T. Synthesis and characterization of layer-by-layer assembled magnesium zinc molybdate nanocontainer for anticorrosive application. Chem. Eng. J. 2016, 295, 414–426. [Google Scholar] [CrossRef]
  42. Yeganeh, M.; Omidi, M.; Rabizadeh, T. Anti-corrosion behavior of epoxy composite coatings containing molybdate-loaded mesoporous silica. Prog. Org. Coat. 2019, 126, 18–27. [Google Scholar] [CrossRef]
  43. Sheng, X.; Zhou, L.; Guo, X.; Bai, X.; Liu, X.; Liu, J.; Luo, C. Composition design and anticorrosion performance optimization of zinc molybdate pigments. Mater. Today Commun. 2021, 28, 102477. [Google Scholar] [CrossRef]
  44. Yan, H.; Wang, J.; Zhang, Y.; Hu, W. Preparation and inhibition properties of molybdate intercalated ZnAlCe layered double hydroxide. J. Alloys Compd. 2016, 678, 171–178. [Google Scholar] [CrossRef]
  45. Sun, Y.; Wang, X.; Ai, Y.; Yu, Z.; Huang, W.; Chen, C.; Hayat, T.; Alsaedi, A.; Wang, X. Interaction of sulfonated graphene oxide with U(VI) studied by spectroscopic analysis and theoretical calculations. Chem. Eng. J. 2017, 310, 292–299. [Google Scholar] [CrossRef]
  46. Seo, D.C.; Jeon, I.; Jeong, E.S.; Jho, J.Y. Mechanical Properties and Chemical Durability of Nafion/Sulfonated Graphene Oxide/Cerium Oxide Composite Membranes for Fuel-Cell Applications. Polymers 2020, 12, 1375. [Google Scholar] [CrossRef] [PubMed]
  47. Xing, X.; Xu, X.; Wang, J.; Hu, W. Preparation and inhibition behavior of ZnMoO4/reduced graphene oxide composite for Q235 steel in NaCl solution. Appl. Surf. Sci. 2019, 479, 835–846. [Google Scholar] [CrossRef]
  48. Xue, R.; Hong, W.; Pan, Z.; Jin, W.; Zhao, H.; Song, Y.; Zhou, J.; Liu, Y. Enhanced electrochemical performance of ZnMoO4/reduced graphene oxide composites as anode materials for lithium-ion batteries. Electrochim. Acta 2016, 222, 838–844. [Google Scholar] [CrossRef] [Green Version]
  49. Chen, Z.; Yang, W.; Xu, B.; Guo, Y.; Chen, Y.; Yin, X.; Liu, Y. Corrosion behaviors and physical properties of polypyrrole-molybdate coating electropolymerized on carbon steel. Prog. Org. Coat. 2018, 122, 159–169. [Google Scholar] [CrossRef]
  50. Hou, H.; Hu, X.; Liu, X.; Hu, W.; Meng, R.; Li, L. Sulfonated graphene oxide with improved ionic performances. Ionics 2015, 21, 1919–1923. [Google Scholar] [CrossRef]
  51. Umar, M.I.A.; Yap, C.C.; Awang, R.; Umar, A.A.; Salleh, M.M.; Yahaya, M. Formation of gold-coated multilayer graphene via thermal reduction. Mater. Lett. 2013, 106, 200–203. [Google Scholar] [CrossRef]
  52. Zhai, B.; Ma, Q.; Yang, L.; Huang, Y. Effects of Sintering Temperature on the Morphology and Photoluminescence of Eu3+ Doped Zinc Molybdenum Oxide Hydrate. J. Nanomater. 2018, 2018, 7418508. [Google Scholar] [CrossRef] [Green Version]
  53. Lu, W.; Wang, D.; Wang, Q.; Yang, F.; Li, T.; Shi, Y.; Zhang, S.; Yang, B. Sensitivity of Corrosion Behavior for Fe-Based Amorphous Coating to Temperature and Chloride Concentration. Coatings 2021, 11, 331. [Google Scholar] [CrossRef]
  54. Wongpanya, P.; Saramas, Y.; Chumkratoke, C.; Wannakomol, A. Erosion–corrosion behaviors of 1045 and J55 steels in crude oil. J. Pet. Sci. Eng. 2020, 189, 106965. [Google Scholar] [CrossRef]
  55. Bhargava, G.; Ramanarayanan, T.A.; Bernasek, S.L. Imidazole-Fe Interaction in an Aqueous Chloride Medium: Effect of Cathodic Reduction of the Native Oxide. Langmuir 2010, 26, 215–219. [Google Scholar] [CrossRef] [PubMed]
  56. Guitián, B.; Nóvoa, X.R.; Pintos, A. Development of conversion coatings on iron via corrosion in LiPF6 solution. Electrochim. Acta 2019, 304, 428–436. [Google Scholar] [CrossRef]
  57. Qiu, S.; Li, W.; Zheng, W.; Zhao, H.; Wang, L. Synergistic Effect of Polypyrrole-Intercalated Graphene for Enhanced Corrosion Protection of Aqueous Coating in 3.5% NaCl Solution. ACS Appl. Mater. Interfaces 2017, 9, 34294–34304. [Google Scholar] [CrossRef] [PubMed]
  58. Liu, Y.; Wang, J.; Liu, L.; Li, Y.; Wang, F. Study of the failure mechanism of an epoxy coating system under high hydrostatic pressure. Corros. Sci. 2013, 74, 59–70. [Google Scholar] [CrossRef]
  59. Yeganeh, M.; Keyvani, A. The effect of mesoporous silica nanocontainers incorporation on the corrosion behavior of scratched polymer coatings. Prog. Org. Coat. 2016, 90, 296–303. [Google Scholar] [CrossRef]
  60. Conradi, M.; Kocijan, A.; Kek-Merl, D.; Zorko, M.; Verpoest, I. Mechanical and anticorrosion properties of nanosilica-filled epoxy-resin composite coatings. Appl. Surf. Sci. 2014, 292, 432–437. [Google Scholar] [CrossRef]
  61. Qiu, S.; Chen, C.; Cu, M.; Li, W.; Zhao, H.; Wang, L. Corrosion protection performance of waterborne epoxy coatings containing self-doped polyaniline nanofiber. Appl. Surf. Sci. 2017, 407, 213–222. [Google Scholar] [CrossRef]
  62. Kathavate, V.S.; Bagal, N.S.; Deshpande, P.P. Corrosion protection performance of nano-TiO2-containing phosphate coatings obtained by anodic electrochemical treatment. Corros. Rev. 2019, 37, 565–578. [Google Scholar] [CrossRef]
  63. Jain, R.; Bhagawati, B.; Khandagiri, P.; Shamshoddin, S.; Bhadu, M.K.; Rout, T.K.; Das, S. Anticorrosive and lubricating polyphenol coatings on galvanneal steel. Surf. Eng. 2016, 33, 410–427. [Google Scholar] [CrossRef]
  64. Bagal, N.S.; Kathavate, V.S.; Deshpande, P.P. Nano-TiO2 Phosphate Conversion Coatings—A Chemical Approach. Electrochem. Energy Technol. 2018, 4, 47–54. [Google Scholar] [CrossRef]
  65. Wang, G.; Wen, S.; Qian, S.; Wang, J.; Wang, C.; Chen, Y. Synthesis of novel nano hyperbranched polymer resin and its corrosion resistance in coatings. Prog. Org. Coat. 2020, 140, 105496. [Google Scholar] [CrossRef]
Figure 1. The schematic illustration of SZMO@SG synthesis.
Figure 1. The schematic illustration of SZMO@SG synthesis.
Coatings 12 01634 g001
Figure 2. FT-IR spectra of SG, ZMO, and SZMO@SG.
Figure 2. FT-IR spectra of SG, ZMO, and SZMO@SG.
Coatings 12 01634 g002
Figure 3. XPS spectra and high resolution XPS spectra of C 1s, O 1s, Zn 2p, Mo 3d, S 2p of (a) SG, (b) ZMO, and (c) SZMO@SG.
Figure 3. XPS spectra and high resolution XPS spectra of C 1s, O 1s, Zn 2p, Mo 3d, S 2p of (a) SG, (b) ZMO, and (c) SZMO@SG.
Coatings 12 01634 g003
Figure 4. XRD patterns for SG, ZMO and SZMO@SG. (The characteristic peak of SG, ZMO and SZMO@SG are marked with symbols).
Figure 4. XRD patterns for SG, ZMO and SZMO@SG. (The characteristic peak of SG, ZMO and SZMO@SG are marked with symbols).
Coatings 12 01634 g004
Figure 5. SEM images of ZMO synthesized at different SG contents. (a) control without SG; (b) 0.3 wt% SG, (c) 0.6 wt% SG.
Figure 5. SEM images of ZMO synthesized at different SG contents. (a) control without SG; (b) 0.3 wt% SG, (c) 0.6 wt% SG.
Coatings 12 01634 g005
Figure 6. Water contact angles of polyurethane coatings with various SZMO@SG dosages in 5 days.
Figure 6. Water contact angles of polyurethane coatings with various SZMO@SG dosages in 5 days.
Coatings 12 01634 g006
Figure 7. Element distribution of O, Na, Cl, Fe, Zn, and Mo of the cross-section of different coatings (a) pure resin before immersion, (b) pure resin immersed in 3.5 wt% NaCl solution for 1008 h, (c) 3 wt% SZMO@SG coatings before immersion and (d) 3 wt% SZMO@SG coatings immersed in 3.5 wt% NaCl solution for 1008 h.
Figure 7. Element distribution of O, Na, Cl, Fe, Zn, and Mo of the cross-section of different coatings (a) pure resin before immersion, (b) pure resin immersed in 3.5 wt% NaCl solution for 1008 h, (c) 3 wt% SZMO@SG coatings before immersion and (d) 3 wt% SZMO@SG coatings immersed in 3.5 wt% NaCl solution for 1008 h.
Coatings 12 01634 g007
Figure 8. The images of (a) coating samples with 3.5 wt% NaCl solution immersion for different times and high resolution XPS spectra of Zn 2p, Mo 3d, Fe 2p of (b) control, (ce) coatings with 3 wt% SZMO@SG immersed in 3.5 wt% NaCl solution for 1008 h.
Figure 8. The images of (a) coating samples with 3.5 wt% NaCl solution immersion for different times and high resolution XPS spectra of Zn 2p, Mo 3d, Fe 2p of (b) control, (ce) coatings with 3 wt% SZMO@SG immersed in 3.5 wt% NaCl solution for 1008 h.
Coatings 12 01634 g008
Figure 9. Potentiodynamic polarization curves of different coatings in 3.5wt% NaCl solution for (a) 48 h, (b) 144 h, and (c) 840 h.
Figure 9. Potentiodynamic polarization curves of different coatings in 3.5wt% NaCl solution for (a) 48 h, (b) 144 h, and (c) 840 h.
Coatings 12 01634 g009
Figure 10. Nyquist plots of different coatings immersed in 3.5 wt% NaCl solution for (a) 48 h, (b) 144 h, and (c) 840 h.
Figure 10. Nyquist plots of different coatings immersed in 3.5 wt% NaCl solution for (a) 48 h, (b) 144 h, and (c) 840 h.
Coatings 12 01634 g010
Figure 11. Bode plots of different coatings immersed in 3.5 wt% NaCl solution for (a) 48 h, (b) 144 h, (c) 840 h.
Figure 11. Bode plots of different coatings immersed in 3.5 wt% NaCl solution for (a) 48 h, (b) 144 h, (c) 840 h.
Coatings 12 01634 g011
Figure 12. Bode plots of different coatings immersed in 3.5 wt% NaCl solution for (a) 48 h, (b) 144 h, and (c) 840 h.
Figure 12. Bode plots of different coatings immersed in 3.5 wt% NaCl solution for (a) 48 h, (b) 144 h, and (c) 840 h.
Coatings 12 01634 g012
Figure 13. The proposed equivalent electrical circuit of coatings according to the impedance data.
Figure 13. The proposed equivalent electrical circuit of coatings according to the impedance data.
Coatings 12 01634 g013
Figure 14. Mechanism diagram of corrosion resistance of coatings with SZMO@SG.
Figure 14. Mechanism diagram of corrosion resistance of coatings with SZMO@SG.
Coatings 12 01634 g014
Table 1. The change in element contents of different coatings with different immersion times.
Table 1. The change in element contents of different coatings with different immersion times.
SamplesO (%)Na (%)Cl (%)Fe (%)Zn (%)Mo (%)
control-0 h38.070.290.2061.390.060.00
control-1008 h39.699.030.2151.070.000.00
3 wt% SZMO@SG-0 h23.860.900.1267.945.590.90
3 wt%
SZMO@SG-1008 h
40.1210.712.4439.865.870.99
Table 2. Tafel electrochemical measurement data of different coatings for different times.
Table 2. Tafel electrochemical measurement data of different coatings for different times.
SamplesTimeEcorr (V)Icorr (×10−3 mA/cm2)ba−bcη (%)
control48 h−0.5866.7110.1662.603-
144 h−0.62810.694.4894.420-
840 h−0.599109.7011.2001.964-
1 wt%
SZMO@SG
48 h−0.5506.915.1304.417−3.0
144 h−0.5988.748.9042.99018.2
840 h−0.58311.638.4873.39789.4
3 wt%
SZMO@SG
48 h−0.4531.714.5812.92174.5
144 h−0.4593.565.3302.99566.7
840 h−0.6827.974.4495.98492.7
5 wt%
SZMO@SG
48 h−0.5193.767.9433.38043.9
144 h−0.57310.0813.8613.2824.9
840 h−0.64611.269.9964.64289.7
Table 3. Electrochemical impedance spectra data of different coatings for different immersion times.
Table 3. Electrochemical impedance spectra data of different coatings for different immersion times.
SamplesTimeRs
(Ω·cm2)
CPEf
−1 s−ncm−2)
nfRf
(Ω·cm2)
CPEdl
−1 s−ncm−2)
ndlRct
(Ω·cm2)
P (%)
control48 h5.01.87 × 10−81.00289.15.26 × 10−50.5286080.75
144 h2.92.64 × 10−60.7199.58.35 × 10−40.6870211.41
840 h3.65.35 × 10−70.9217.99.48 × 10−40.5121953.43
1 wt%
SZMO@SG
48 h4.02.55 × 10−80.96310.97.29 × 10−60.7157300.78
144 h3.41.80 × 10−81.00173.81.45 × 10−40.5049641.46
840 h5.21.29 × 10−81.00483.62.12 × 10−40.4674050.82
3 wt%
SZMO@SG
48 h3.72.42 × 10−91.003201.04.01 × 10−60.56283,1000.01
144 h6.41.38 × 10−80.93819.04.08 × 10−50.56104,5000.02
840 h4.99.05 × 10−80.94127.51.97 × 10−40.5651,9100.32
5 wt%
SZMO@SG
48 h4.53.46 × 10−81.00110.22.73 × 10−60.8220,8700.17
144 h5.52.02 × 10−70.8949.65.02 × 10−40.5277860.75
840 h5.73.38 × 10−91.0011246.21 × 10−50.6414214.68
Publisher’s Note: MDPI stays neutral with regard to jurisdictional claims in published maps and institutional affiliations.

Share and Cite

MDPI and ACS Style

Zhao, Z.; Chen, K.; Wen, S.; Wang, J.; Xu, J.; Wang, S.; Li, W.; Song, J. Preparation of Zn5Mo2O11·5H2O@Sulfonated Graphene by Template Method and Its Anticorrosion Mechanism in Polyurethane Coatings. Coatings 2022, 12, 1634. https://doi.org/10.3390/coatings12111634

AMA Style

Zhao Z, Chen K, Wen S, Wang J, Xu J, Wang S, Li W, Song J. Preparation of Zn5Mo2O11·5H2O@Sulfonated Graphene by Template Method and Its Anticorrosion Mechanism in Polyurethane Coatings. Coatings. 2022; 12(11):1634. https://doi.org/10.3390/coatings12111634

Chicago/Turabian Style

Zhao, Zihao, Kaimin Chen, Shaoguo Wen, Jihu Wang, Jinglu Xu, Song Wang, Weiping Li, and Jia Song. 2022. "Preparation of Zn5Mo2O11·5H2O@Sulfonated Graphene by Template Method and Its Anticorrosion Mechanism in Polyurethane Coatings" Coatings 12, no. 11: 1634. https://doi.org/10.3390/coatings12111634

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.

Article Metrics

Back to TopTop