Next Article in Journal
A Method of Ore Blending Based on the Quality of Beneficiation and Its Application in a Concentrator
Previous Article in Journal
Production, Optimization and Characterization of Polylactic Acid Microparticles Using Electrospray with Porous Structure
Previous Article in Special Issue
Low-Temperature and Low-Pressure Silicon Nitride Deposition by ECR-PECVD for Optical Waveguides
 
 
Font Type:
Arial Georgia Verdana
Font Size:
Aa Aa Aa
Line Spacing:
Column Width:
Background:
Article

Enhancing the Photoluminescence and Microstructural Transformations of Al2O3/Glass–Ceramic Composite Coatings by Laser Irradiation

1
Semillero de Investigación en Materiales para Sistemas Energéticos Sostenibles, Universidad Autónoma de Occidente, 760030 Cali, Colombia
2
Grupo de Optoelectrónica, Instituto Interdisciplinario de las Ciencias, Universidad del Quindío, 630002 Armenia, Colombia
3
Grupo de Metalurgia Física y Teoría de Transiciones de Fase GMTF, Universidad del Valle, 760032 Cali, Colombia
4
Grupo de Transiciones de Fase y Materiales Funcionales, Centro de Excelencia en Nuevos Materiales (CENM), Universidad del Valle, 760032 Cali, Colombia
5
IFN-CNR CSMFO Laboratory and FBK Photonics Unit, Povo, 38123 Trento, Italy
6
Grupo de Ciencia e Ingeniería de Materiales, Universidad Autónoma de Occidente, 760030 Cali, Colombia
*
Author to whom correspondence should be addressed.
Appl. Sci. 2021, 11(11), 5091; https://doi.org/10.3390/app11115091
Submission received: 28 February 2021 / Revised: 28 March 2021 / Accepted: 30 March 2021 / Published: 31 May 2021
(This article belongs to the Special Issue Photonic Glass-Ceramics: Fabrication, Properties and Applications)

Abstract

:
This work presents an analysis of the crystallization process and the influence of laser surface modification on the crystalline phases and optical responses of Al2O3/glass–ceramic coatings deposited on a brass substrate. We used a CO2 laser at different irradiation powers to change the structure of the superficial layer. The photoluminescence response enhanced the resolution of its line shape as the irradiation power increased. X-ray diffraction patterns exhibit the presence of different crystalline phases for the samples irradiated.

1. Introduction

Alumina ceramics have found, for a long time, several important technological applications in optical [1] and microelectronic components [2] as protective, decorative, wear-resistant, solid-state device applications [3,4] and anticorrosion coatings [5,6,7], due to their chemical inertness, good mechanical strength and high hardness, transparency and good insulating properties [8].
In particular, high-temperature applications represent a new challenge for alumina ceramic joints in many fields [9], especially for complex-shaped alumina ceramic components. It has been found that joining ceramics to themselves, or to metals, can be achieved by direct solid-state diffusion [10], joining with metallic interlayers [11] and joining using glass or glass–ceramic interlayers [9,12,13]. These processes depend on solid-state diffusion and the interface that is formed at high pressures and high temperatures. A high bonding temperature, high bonding load and excellent surface finish [9] are generally required for joining ceramics. Some problems reported are the low resistance to oxidation at high temperatures, in addition to relatively long processing times at high temperatures to ensure sufficient mutual diffusion.
Joining with glass and glass–ceramic fillers is more appropriate due to the excellent chemical compatibility and matched coefficient of thermal expansion (CTE) between glass filler and ceramics [9,12,14]. CaO-Al2O3-SiO2 have been employed as fillers for joining alumina ceramics [15]. On the other hand, CaO-Al2O3-SiO2-TiO2 glass ceramics are also used [9]. Among the advantages of using glass ceramics is the ability to obtain higher crystallinity, which allows the joint to be used at higher temperatures.
Several studies address the silica-stabilized zirconia, SiO2-ZrO2 glass–ceramic system, synthesized with the sol–gel method [16,17] and, like alumina, its applications are aimed at taking advantage of its thermal and optical properties, especially in thermal barrier coatings. To study new materials for joining alumina ceramics and new procedures, this work uses SiO2-ZrO2 glass–ceramic fillers and a CO2 laser surface modification technique. The use of laser surface treatment techniques for the treatment of alumina coatings has been reported due to the high crystallinity that it confers on the material, and it has been shown that the required time is usually in the range of 1 to 15 min [15]. Further, laser treatment represents an optical technique to detect phase transformation and densification of Al2O3 coatings. Laser surface modification of alumina coatings leads to the elimination of porosities and restoration of the stable phase [3,18].
This paper reports the spectroscopic properties of the Al2O3/SiO2-ZrO2 glass–ceramic filler on the brass substrate, where the laser surface modification causes a phase transformation.

2. Materials and Methods

The Al2O3/glass–ceramic composite coating was deposited onto brass substrates by the sol–gel process. Before deposition of the glass ceramic, an alumina interlayer (Al2O3) was deposited over the brass substrate using the standard air plasma spray technique to ensure the junction of the glass–ceramic layer. The brass substrates were cleaned by ultra-sound and alcohol without any special surface treatment. To achieve uniform porosity networks, we used a fused and crushed alumina powder (Metco 105&105SF).
For the preparation of the ZrO2-SiO2 glass ceramic, silica was synthesized via acid hydrolysis of traethylorthosilicate (TEOS, Merck 98% purity), ethanol (Sigma-Aldrich, 99.5% purity), de-ionized water (Amresco) and nitric acid as the catalyzer. The mixture was pre-hydrolyzed for 1 h at 70 °C, and it was maintained under these conditions for another 3 h to induce gelation. The molar ratio of TEOS:HNO3:EtOH:H2O was 0.1:0.00005:15.5:2.8. Pure zirconia was obtained from hydrolysis of two different precursors, Zr(C3H7O)4 (Sigma-Aldrich) and ZrClO2·8H2O (Merck). The mixture was kept at 50 °C for 1 h under constant agitation. This suspension was then added to the TEOS solution, resulting in a Zr:Si molar ratio of 90:10, and maintained at 70 °C for 1 h. The preparation was deposited onto Al2O3/brass substrates (1 in diameter) by the spin-coating technique (Laurell technologies ws-650 series). We established the rotation speed at 500 rpm and the rotation time at 50 s.
The Al2O3/ZrO2-SiO2 composite coating deposited on the brass substrate was then thermally treated at 850 °C for 60 min. Three samples were stabilized by a post-treatment using a CO2 laser. This laser (Boye Laser HSLC-1206) of 10.6 µm wavelength with a beam diameter of 6 mm was used for laser modification of the surface. The power density of the CO2 laser beam was 0.69 (SSZ01), 1.04 (SSZ02) and 1.38 W/cm2 (SSZ03). The samples were positioned at around 50 cm from the laser output and exposed for 1 min. In Figure 1, we present the computer-aided design (CAD) for the laser annealing path (1 in2).
The photoluminescent signal was obtained by exciting the sample with the 488 nm line of an Argon laser. A 1 m focal distance spectrometer, with an 1800 g/mm grating and a thermoelectrically cooled CCD camera, was used to analyze the spectral response. The range for photoluminescence (PL) signal detection was between 550 and 900 nm.
The crystalline structure of the sample was investigated by X-ray diffraction (XRD). The diffractometer used was a Bruker D8 Advance with a vertical goniometer; the emission used was 1.5 angstrom radiation emitted by a Cu anode (Kα line) using 35 mA for the filament current and 30 kV for electron acceleration. The detector was a NaI crystal coupled to a photomultiplier tube. A graphite monochromator was located before the detector to eliminate the Cu-Kβ line. The divergence and antiscattering slits used were 0.6 mm each and 0.1 mm for the detector slit. The microstructure of the samples was studied using a scanning electron microscope (SEM, Phenom PROX, Cali, Colombia).

3. Results and Discussion

With the methodology described previously, we obtained regular coatings for all the thermally treated and laser-irradiated samples. The surface micrographs of the Al2O3/glass–ceramic coating are shown in Figure 2. The path laser is evident in the laser annealing surfaces. The laser path’s definition on the surface is higher for higher laser density power (Figure 2c).
Figure 3 shows the surface morphology of the SSZ03 sample. The SEM images reveal a change in the surface profile created after laser irradiation on the Al2O3/glass–ceramic coating. The glass ceramic resembles a kind of broken glass on top of the alumina film. The coating layer’s morphology is not uniform in the microscopic range, and the cracked surface is probably due to differences in the thermal behavior. The thickness of the alumina coating with similar manufacturing parameters is between 400 and 500 μm, as shown in Figure 4, in which the same authors have used Inconel 718 alloy as a substrate.
The SEM micrograph presented in Figure 5a corresponds to the surface image over the Al2O3/glass–ceramic coating. In two different positions on the surface, the composition is described by the EDS spectra (Figure 5b,c). It is evidenced that position 1 corresponds to the Al2O3 layer and position 2 to ZrO2-SiO2.
Figure 6a corresponds to an image of a sample surface annealed by irradiation using 1.38 W/cm2 of laser power density and following the design mentioned above. The surface exhibits differences between sections which are irradiated and those not irradiated. The modifications induced by the laser are structural, and the thermo-optic response supports this statement. Figure 6b shows the image obtained from the infrared emission induced by 520 nm radiation. In this map, the path pattern of the laser can be observed, showing the differences between the irradiated areas, as well as the homogeneity in the laser treatment carried out. This signal is associated with different non-radiative mechanisms and heat diffusion capabilities.
X-ray diffraction patterns of Al2O3/SiO2-ZrO2 and Al2O3 coatings both deposited on the brass substrate are presented in Figure 7. Figure 7a showed traces of tetragonal zirconia crystals at 30.2°, 50.4°, 50.7° (2θ) reported in the JCPDS-ICDD data (set no. 50-1089). The tetragonal ZrO2 diffraction peaks correspond to the crystalline planes (011), (112) and (020), respectively, and the phase is conserved even when the sample reaches room temperature. Like the yttria-stabilized zirconia (YSZ), the most common material used as the ceramic layer, this demonstrates the well-known stabilizing effect in the ZrO2 structure, promoting the formation of high-purity tetragonal zirconia [19,20,21]. On the other hand, although the Al2O3/brass substrate sample displayed both α-brass and β-brass phases, compared with the Al2O3/SiO2-ZrO2/brass substrate, only α-brass was still observed [22]. This indicates that the β-brass is present or formed when the Al2O3 is deposited (γ-Al2O3), and when glass–ceramic and thermal treatment are used, this phase is transformed into α-brass.
Figure 8 shows the X-ray diffraction patterns for the Al2O3/glass–ceramic composite coating system with different post-annealing treatments. Figure 8a shows only the sample annealed at 850 °C at 60 min without any laser post-annealing; Figure 8b shows the sample annealed at 850 °C at 60 min and under a CO2 laser using 0.69 W/cm2 power density for 1 min; Figure 8c shows the sample annealed at 850 °C and under a CO2 laser using 1.04 W/cm2 power density for 1 min. All spectra display evidence of ZrO2 formation, which is stable at ambient temperature. It is important to note that it was possible to obtain stable tetragonal ZrO2 in the SiO2-ZrO2 coating by spin-coating and the thermal treatment applied at 850 °C for 60 min. The fitting procedure of the diffractograms indicates that the dominant structure is the tetragonal phase for ZrO2, especially when CO2 laser irradiation energy is increased (to see 2θ = 30.2°).
The sample annealed at 850 °C for 60 min (Figure 8a) in the oven shows differences from the same sample with CO2 laser post-annealing using 0.69 W/cm2 (Figure 8b) and 1.04 W/cm2 (Figure 8c) power density for 1 min. In Figure 8a, the as-sprayed γ-Al2O3 is in a metastable phase, which is due to the rapid cooling rate of the process of plasma spraying, wherein alumina powder injected into the high temperature plasma is melted and entrained in the gas stream and is then accelerated and impinges on the substrate to form the coating [23]. CO2 laser annealing allows the transformation of γ-Al2O3 into thermodynamically stable α-Al2O3, this transformation being more visible at higher power densities. Figure 8b,c show the XRD patterns typical of the stable corundum structure reported in JCPDS-ICDD data (set no. 46-1212).
Figure 9 shows the PL spectra of SiO2-ZrO2/Al2O3 coatings without laser post-annealing and annealed for 1 min with different laser power densities: 0.69, 1.04, 1.38 W/cm2. In this figure, the effect of laser power on the optical response is shown. All annealed samples exhibit a doublet at around 694 nm and broad and weak emission bands at lower energies, in which intensities and sharpness are enhanced as the laser power increases. The origin of these emission bands is not yet established. We found reports that the spectral emission at higher energies is due to the F+ center (330 and 415 nm). Chromium impurity in the Al2O3 lattice is characterized by two bands of absorption (3.1 and 2.2 eV), and one sharp emission structure peaked at 1.8 eV (696 nm), quite near the emission peak obtained by PL in this work [4,22]. According to this report, for the materials involved in the Al2O3/glass–ceramic composite coatings, the PL emission is associated with silica and zirconia in the Al2O3 bond coat.

4. Conclusions

In this paper, we report the crystallization and the influence of laser surface modification on the crystalline phases and optical response of Al2O3/glass–ceramic coatings. The ZrO2-SiO2 glass ceramic on alumina coatings prepared using the sol–gel technique, deposited under the experimental conditions used in this study, can be used for applications where a more stable alpha-alumina structure is required. This is due to the zirconia incorporated in the system maintaining its tetragonal phase at room temperature. This stable tetragonal ZrO2 phase at room temperature was obtained using annealing in an oven at 850 °C in the Al2O3/SiO2-ZrO2 composite coating.
Additionally, the results show that the use of CO2 laser annealing allows the identification of the spectroscopic properties of the studied system. In this sense, different power densities of 0.69 W/cm2, 1.04 W/cm2 and 1.38 W/cm2 were used to identify these properties. The annealing for 1 min allows the photoluminescence of the glass–ceramic system with optical emission to exhibit an intense double peak at 693 nm (1.789 eV) and 694 nm (1.786 eV) and weaker emission at lower energies. According to the surface micrographs and EDS analysis, the optical response is probably due to Al2O3, with a weak contribution of the ZrO2-SiO2 glass ceramic at lower energies. Although the study had a very important focus on the phase transformation of alumina associated with heat treatment in furnaces and lasers, it can be shown that the entire studied system has a good response to CO2 laser annealing, since emission is well defined; thus, it could be of interest for various optical applications.

Author Contributions

Conceptualization, C.G.; methodology, J.C., J.M., J.J. and L.G.; investigation J.C.; formal analysis, L.T., H.C., J.E.D.; validation, A.C.; supervision, C.G.; resources, C.G., L.T., H.C., J.E.D. and A.C.; data curation, C.G.; writing—original draft preparation, C.G., L.T. and A.C.; writing—review and editing, C.G.; visualization, L.T. and A.C.; supervision, C.G.; project administration, C.G.; funding acquisition, C.G. All authors have read and agreed to the published version of the manuscript.

Funding

This research received no external funding.

Institutional Review Board Statement

Not applicable.

Informed Consent Statement

Not applicable.

Data Availability Statement

Not applicable.

Acknowledgments

The authors are grateful to the IIC radiometry laboratory of Universidad del Quindío and the Universidad Autónoma de Occidente for funding (Project code No. 17INTER-289).

Conflicts of Interest

The authors declare no conflict of interest.

References

  1. Aabid, A.; Khan, S.A. Optimization of Heat Transfer on Thermal Barrier Coated Gas Turbine Blade. IOP Conf. Ser. Mater. Sci. Eng. 2018, 370, 012022. [Google Scholar] [CrossRef]
  2. Sankar, V.; Ramkumar, P.B.; Sebastian, D.; Joseph, D.; Jose, J.; Kurian, A. Optimized Thermal Barrier Coating for Gas Turbine Blades. Mater. Today Proc. 2019, 11, 912–919. [Google Scholar] [CrossRef]
  3. Ghosh, S. Thermal properties of glass-ceramic bonded thermal barrier coating system. Trans. Nonferrous Met. Soc. China 2015, 25, 457–464. [Google Scholar] [CrossRef]
  4. Adachi, S. Luminescence spectroscopy of Cr3+ in Al2O3 polymorphs. Opt. Mater. 2021, 114, 111000. [Google Scholar] [CrossRef]
  5. Liu, B.; Liu, Y.; Zhu, C.; Xiang, H.; Chen, H.; Sun, L.; Gao, Y.; Zhou, Y. Advances on strategies for searching for next generation thermal barrier coating materials. J. Mater. Sci. Technol. 2019, 35, 833–851. [Google Scholar] [CrossRef]
  6. Masalski, J.; Gluszek, J.; Zabrzeski, J.; Nitsch, K.; Gluszek, P. Improvement in corrosion resistance of the 316l stainless steel by means of Al2O3 coatings deposited by the sol-gel method. Thin Solid Films 1999, 349, 186–190. [Google Scholar] [CrossRef]
  7. Cao, X.Q.; Vessen, R.; Stoever, D. Ceramic materials for thermal barrier coatings. J. Eur. Ceram. Soc. 2004, 24, 1–10. [Google Scholar] [CrossRef]
  8. Guidi, F.; Moretti, G.; Carta, G.; Natali, M.; Rossetto, G.; Pierino, Z.; Salmaso, G.; Rigato, V. Electrochemical anticorrosion performance evaluation of Al2O3 coatings deposited by MOCVD on an industrial brass substrate. Electrochim. Acta 2005, 50, 4609–4614. [Google Scholar] [CrossRef]
  9. Zhu, W.; Zhang, H.; Xue, D.; Jiang, H.; Ran, X. Joining alumina ceramic by using glass ceramic filler with high crystallinity for high temperature application. Ceram. Int. 2019, 45, 20999–21003. [Google Scholar] [CrossRef]
  10. Nagano, T.; Kato, H. Difussion bonding of Zirconia/Alumina composites. J. Am. Chem. Soc. 1990, 73, 3476–3480. [Google Scholar]
  11. Valette, C.; Marie-Francoise, D.; Voytovych, R.; Eustathopoulos, N. Interfacial reactions in alumina/CuAgTi braze/CuNi system. Interfacial reactions in alumina/CuAgTi braze/CuNi system. Scr. Mater. 2005, 52, 1–6. [Google Scholar] [CrossRef]
  12. Wang, G.; Shan, Y.; Xu, J.; Chen, Y.; Li, J. Joining of AlON ceramics by using β-SiAlON/Y-Si-Al-O-N glass-ceramic as interlayer. J. Non Cryst. Solids 2019, 503, 389–396. [Google Scholar] [CrossRef]
  13. Menzler, N.H.; Bram, M.; Buchkremer, H.P.; Stöver, D. Development of a gastight sealing material for ceramic components. J. Eur. Ceram. Soc. 2003, 23, 445–454. [Google Scholar] [CrossRef]
  14. Döhler, F.; Kasch, S.; Schmidt, T.; Rüssel, C. Sealing of alumina using a CO2 laser and a rapidly crystallizing glass. J. Mater. Process. Technol. 2016, 233, 206–211. [Google Scholar] [CrossRef]
  15. Esposito, L.; Bellosi, A. Ceramic oxide bonds using calcium aluminosilicate glasses. J. Mater. Sci. 2005, 48, 2493–2498. [Google Scholar] [CrossRef]
  16. Miranda-Salvado, I.M.; Serna, C.J.; Fernandez-Navarro, J.M. ZrO2-SiO2 materials prepared by sol-gel. J. Non Cryst. Solids 1988, 330, 100. [Google Scholar] [CrossRef]
  17. Wang, S.W.; Huang, X.X.; Guo, J.K. Mechanical properties and microstructure of ZrO2–SiO2 composite. J. Mater. Sci. 1997, 32, 197. [Google Scholar] [CrossRef]
  18. Thirumalaikumarasamy, D.; Shanmugam, K.; Balasubramanian, V. Corrosion performance of atmospheric plasma sprayed alumina coatings on AZ31B magnesium alloy under immersion environment. J. Asian Ceram. Soc. 2014, 2, 403–415. [Google Scholar] [CrossRef]
  19. Goyes, C.; Ferrari, M.; Armellini, C.; Chiasera, A.; Jestin, Y.; Righini, G.C.; Fonthal, F.; Solarte, E. CO2 laser annealing on erbium-activated glass–ceramic waveguides for photonics. Opt. Mater. 2009, 31, 1310–1314. [Google Scholar] [CrossRef]
  20. Torres-Rodríguez, J.; Kalmár, J.; Menelaou, M.; Čelko, L.; Dvořak, K.; Cihlář, J.; Cihlař, J., Jr.; Kaiser, J.; Győri, E.; Veres, P.; et al. Heat treatment induced phase transformations in zirconia and yttria stabilized zirconia monolithic aerogels. J. Supercrit. Fluids 2019, 149, 54–63. [Google Scholar] [CrossRef]
  21. Carpio, P.; Salvador, M.D.; Borrell, A.; Sánchez, E. Thermal behaviour of multilayer and functionally-graded YSZ/Gd2Zr2O7 coatings. Ceram. Int. 2017, 43, 4048–4054. [Google Scholar] [CrossRef] [Green Version]
  22. Ghamnia, M.; Jardin, C.; Bouslama, M. Luminescent centres F and F+ in α-alumina detected by cathodoluminescence technique. J. Electron Spectrosc. Relat. Phenom. 2003, 133, 55. [Google Scholar] [CrossRef]
  23. Krishnan, R.; Dash, S.; Babu Rao, C.; Subba Rao, R.V.; Tyagi, A.K.; Raj, B. Laser induced structural and microstructural transformations of plasma sprayed Al2O3 coatings. Scr. Mater. 2001, 45, 693–700. [Google Scholar] [CrossRef]
Figure 1. Computer-aided design image of the channel written with CO2 laser system.
Figure 1. Computer-aided design image of the channel written with CO2 laser system.
Applsci 11 05091 g001
Figure 2. Imaging of the Al2O3/glass–ceramic composite coating, treated with different power densities of CO2 laser irradiation: (a) without irradiation, (b) 0.69 W/cm2 and (c) 1.04 W/cm2.
Figure 2. Imaging of the Al2O3/glass–ceramic composite coating, treated with different power densities of CO2 laser irradiation: (a) without irradiation, (b) 0.69 W/cm2 and (c) 1.04 W/cm2.
Applsci 11 05091 g002
Figure 3. Scanning electron microscope (SEM) micrographs of the SSZ03 sample at different magnifications: (a) 480× and (b) 1620×.
Figure 3. Scanning electron microscope (SEM) micrographs of the SSZ03 sample at different magnifications: (a) 480× and (b) 1620×.
Applsci 11 05091 g003
Figure 4. SEM micrographs of the alumina SEM image of alumina deposited on Inconel 718.
Figure 4. SEM micrographs of the alumina SEM image of alumina deposited on Inconel 718.
Applsci 11 05091 g004
Figure 5. (a) SEM micrograph of the SSZ03 sample presenting position 1 and 2 for further EDS analysis, (b,c) EDS analysis over two different positions (1 and 2), respectively.
Figure 5. (a) SEM micrograph of the SSZ03 sample presenting position 1 and 2 for further EDS analysis, (b,c) EDS analysis over two different positions (1 and 2), respectively.
Applsci 11 05091 g005
Figure 6. Surface morphology of the SSZ03 sample with laser annealing using 1.38 W/cm2 of power density: (a) optical microscopy image and (b) mapping of infrared emission induced by 520 nm radiation.
Figure 6. Surface morphology of the SSZ03 sample with laser annealing using 1.38 W/cm2 of power density: (a) optical microscopy image and (b) mapping of infrared emission induced by 520 nm radiation.
Applsci 11 05091 g006
Figure 7. XRD pattern of (a) Al2O3/SiO2-ZrO2 composite coating deposited on brass substrate annealed at 850 °C; (b) Al2O3 interlayer on brass substrate.
Figure 7. XRD pattern of (a) Al2O3/SiO2-ZrO2 composite coating deposited on brass substrate annealed at 850 °C; (b) Al2O3 interlayer on brass substrate.
Applsci 11 05091 g007
Figure 8. XRD pattern of Al2O3/glass–ceramic coating on CuZn substrate. (a) Only annealed at 850 °C at 60 min without any laser post-annealing; (b) annealed at 850 °C at 60 min and under CO2 laser using 0.69 W/cm2 power density for 1 min; (c) annealed at 850 °C and under CO2 laser using 1.04 W/cm2 power density for 1 min.
Figure 8. XRD pattern of Al2O3/glass–ceramic coating on CuZn substrate. (a) Only annealed at 850 °C at 60 min without any laser post-annealing; (b) annealed at 850 °C at 60 min and under CO2 laser using 0.69 W/cm2 power density for 1 min; (c) annealed at 850 °C and under CO2 laser using 1.04 W/cm2 power density for 1 min.
Applsci 11 05091 g008
Figure 9. Photoluminescence spectra of SiO2-ZrO2 with CO2 laser post-annealing for 1 min, using a power density of (a) 0.69 W/cm2; (b) 1.04 W/cm2 and (c) 1.38 W/cm2.
Figure 9. Photoluminescence spectra of SiO2-ZrO2 with CO2 laser post-annealing for 1 min, using a power density of (a) 0.69 W/cm2; (b) 1.04 W/cm2 and (c) 1.38 W/cm2.
Applsci 11 05091 g009
Publisher’s Note: MDPI stays neutral with regard to jurisdictional claims in published maps and institutional affiliations.

Share and Cite

MDPI and ACS Style

Correa, J.; Murillo, J.; Jurado, J.; García, L.; Tirado, L.; Colorado, H.; Diosa, J.E.; Chiasera, A.; Goyes, C. Enhancing the Photoluminescence and Microstructural Transformations of Al2O3/Glass–Ceramic Composite Coatings by Laser Irradiation. Appl. Sci. 2021, 11, 5091. https://doi.org/10.3390/app11115091

AMA Style

Correa J, Murillo J, Jurado J, García L, Tirado L, Colorado H, Diosa JE, Chiasera A, Goyes C. Enhancing the Photoluminescence and Microstructural Transformations of Al2O3/Glass–Ceramic Composite Coatings by Laser Irradiation. Applied Sciences. 2021; 11(11):5091. https://doi.org/10.3390/app11115091

Chicago/Turabian Style

Correa, Julio, Jairo Murillo, Javier Jurado, Lina García, Liliana Tirado, Hernán Colorado, Jesús Evelio Diosa, Alessandro Chiasera, and Clara Goyes. 2021. "Enhancing the Photoluminescence and Microstructural Transformations of Al2O3/Glass–Ceramic Composite Coatings by Laser Irradiation" Applied Sciences 11, no. 11: 5091. https://doi.org/10.3390/app11115091

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.

Article Metrics

Back to TopTop