Next Article in Journal
Sensitivity Analysis in the Modelling of a High Speed Steel Thin-Wall Produced by Directed Energy Deposition
Next Article in Special Issue
Enhanced Cementation of Co2+ and Ni2+ from Sulfate and Chloride Solutions Using Aluminum as an Electron Donor and Conductive Particles as an Electron Pathway
Previous Article in Journal
Effect of Microstructure on Corrosion Behavior of WE43 Magnesium Alloy in As Cast and Heat-Treated Conditions
Previous Article in Special Issue
Evaluation of the Use of Electric Arc Furnace Slag and Ladle Furnace Slag in Stone Mastic Asphalt Mixes with Discarded Cellulose Fibers from the Papermaking Industry
 
 
Font Type:
Arial Georgia Verdana
Font Size:
Aa Aa Aa
Line Spacing:
Column Width:
Background:
Article

Recovery of Cobalt from the Residues of an Industrial Zinc Refinery

1
Department of Mining, Metallurgical and Materials Engineering, Université Laval, Québec, QC G1V 0A6, Canada
2
Institut de Recherche sur les Mines et l’Environnement, Université du Québec en Abitibi Témiscamingue (UQAT), Rouyn-Noranda, QC J9X 5E4, Canada
3
Institut de Recherche, Hydro-Québec, Varennes, QC J3X 1S1, Canada
*
Author to whom correspondence should be addressed.
Metals 2020, 10(11), 1553; https://doi.org/10.3390/met10111553
Submission received: 4 November 2020 / Revised: 18 November 2020 / Accepted: 19 November 2020 / Published: 22 November 2020
(This article belongs to the Special Issue Recovery and Recycling of Valuable Metals)

Abstract

:
The electrolytic production of metallic zinc from processing zinc sulfide concentrates generates a residue containing cadmium, copper, and cobalt that need to be removed from the electrolytic zinc solution because they are harmful to the zinc electro-winning process. This residue is commonly sent to other parties that partly recover the contained elements. These elements can generate revenues if recovered at the zinc plant site. A series of laboratory tests were conducted to evaluate a method to process a zinc plant residue with the objective of recovering cobalt into a salable product. The proposed process comprises washing, selective leaching, purifying and precipitation of cobalt following its oxidation. The process allows the production of a cobalt rich hydroxide precipitate assaying 45 ± 4% Co, 0.8 ± 0.2% Zn, 4.4 ± 0.7% Cu, and 0.120 ± 0.004% Cd at a 61 ± 14% Co recovery. Replicating the whole process with different feed samples allowed the identification of the critical steps in the production of the cobalt product; one of these critical steps being the control of the oxidation conditions for the selective precipitation step.

1. Introduction

The conventional roast-leach zinc extraction process yields a solid residue consisting of a mixture of zinc, copper, cadmium, and cobalt. Some zinc smelting plants process that residue [1,2,3] to recover the contained valuable metals. The high value of cobalt makes it an excellent candidate for a first step in the development of a process to recover the metals contained in that residue [1]. Indeed, cobalt is currently considered as a critical material [4] as it is used in the making of Li-ion batteries [1,5], increasingly strategic for the shift toward green energy or more precisely toward a 100% electric vehicle market [4]. The «critical» status of cobalt is related to uncertainties about the supply of the metal. In fact, 60% of the world’s cobalt is mined in the Congo and 80% of its production is processed in China [4]. In the case of a cobalt supply disruption due to a natural disaster, a change of government or a boycott [6], a zinc residue that contains more than 2% Co [1] becomes an interesting alternative to primary cobalt.
The extraction of cobalt from zinc plant residues is not discussed in many papers except in a recent review [1]. Few papers [2,3,7,8] were found to describe processes to recover cobalt from zinc residues. Wang and Zhou described a process [2] to treat a zinc residue containing active carbon and organic compounds used to capture the cobalt and the manganese from the zinc solution prior to the Zn electro-winning step. The process developed for that residue consists of a washing stage followed by two roasting steps at different temperatures, leaching, and precipitation of iron and manganese followed by anion exchange and solvent extraction of cobalt using extractant P507. Fattahi et al. described a process [3] to extract cobalt from the zinc residues of Iranian Zn smelters that add permanganate to the zinc solution in order to oxidize Co(II) to Co(III) which is precipitated by increasing the pH. The precipitated zinc residue contains about 2% Co and more than 10% Mn. The authors [3] propose a reductive leaching followed by a precipitation of cobalt sulfide (CoS) using Na2S to selectively recover the cobalt from the manganese. Although the conventional approach for the purification of zinc solution is the cementation of Cu, Cd, and Co onto zinc dust [1,9], it was not possible to find in the Western literature a process dedicated to the treatment of this type of residue, although a qualitative description of a possible process can be found in [1]. Li et al. [10] studied the rate of leaching of a zinc residue but did not indicate if the residue is obtained by cementation on zinc dust and the authors did not attempt to process the leach solution to obtain a salable cobalt product.
This paper describes a processing scheme to produce a cobalt rich compound from a zinc plant residue produced by the cementation process. The objective of the test work presented in this paper is not to optimize an existing flowsheet but to propose a process to obtain a salable cobalt compound from a zinc residue produced by cementation on zinc dust. As requested by the industrial partner, the proposed process should use only open tank reactors for leaching and precipitation without resorting to solvent extraction nor ion exchange to obtain the cobalt product. This last constraint complicates the process to be developed as selective extractants are available for cobalt [1,7]. However, if the economics of the process are not favorable, the use of SX will be investigated but it is unlikely that the addition of a SX plant could move the process economics toward more profitable conditions.

2. Materials and Methods

2.1. Instrumentation and Reagents

The solid and liquid samples are assayed using a MP-AES 4200 (microwave-plasma atomic emission spectrometer) from Agilent Technology (Santa Clara, CA, USA). For solid samples, 0.5 g sub samples are taken and digested in aqua regia for analysis using the MP-AES. The pH and Eh of the solution are, respectively, measured using a Fisher Scientific accumet XL600 pH-meter (Waltham, MA, USA), an Orion pH probe, and an Orion Oxidation Reduction Potential (ORP) probe from Thermo scientific (Waltham, MA, USA). Table 1 presents the reagents used for the experimentation.

2.2. Provenance of the Zinc Residue

The zinc residue used for the test work is provided by the CEZinc refinery [11] in Valleyfield, QC, Canada. Figure 1 shows the zinc extraction process and identifies the origin of the Co-bearing zinc residue. The plant processes zinc sulfide concentrates assaying more than 50% Zn, 0–5% Pb, less than 2% Cu, 0.5% Cd and from 50–200 g/t Co. The main impurities are iron (>8%) and sulfur (>30%). The extraction process of zinc begins by a roasting of the zinc sulfide concentrate to oxidize sulfur into SO2 that is subsequently converted into sulfuric acid (H2SO4). The roasting also transforms the zinc sulfide into zinc oxide which is soluble in weakly acidic solutions. The roasted product is leached in sequence with weak and strong sulfuric acid to solubilize the zinc oxide. The metallic impurities (Fe, Cu, Cd, Co) follow the zinc into the solution. The solution then undergoes a neutralization, during which the solubilized iron is precipitated as jarosite [8]. The purification of the iron-free solution from the remaining metallic impurities is done using cementation on zinc dust [9] where copper, cadmium, and cobalt displace the zinc of the zinc powder through the reaction:
M a q 2 + + Zn s Zn a q 2 + + M s
where M stands for copper, cadmium, or cobalt. The reduced copper, cadmium, and cobalt are plated onto the surface of the zinc powder. The cemented powder is separated from the solution by a leaf press filter. The recovered solid is the «Zinc Plant Residue» (ZPR) considered in the following study. This residue is currently transferred to another plant for further processing. Zinc is finally electro-won from the purified solution (See Figure 1). The spent electrolyte is recycled back to the leaching step.

2.3. Characterization of the Zinc Plant Residue (ZPR)

A 20 kg sample of ZPR was collected by the CEZinc personnel at the discharge of the press filter. The sample was shipped wet to the laboratory for the test work. The received sample was split wet into ten parts after spreading the material onto a plastic sheet. One 2 kg sample was put in an oven for drying overnight and the remaining material was kept wet for the subsequent test work. A portion of the dried sample is shown in Figure 2a. The material is strongly agglomerated with practically unbreakable lumps. Sulfuric acid and sulfates are likely responsible for the observed particles binding. It rapidly appeared that this material could not be characterized (chemical composition, size distribution, etc.) as is and it was decided to wash the residue in water to remove any excess of sulfuric acid before drying. Washing was carried out by mixing 500 g of wet residue in 2700 mL of water (15% solids in mass) in a beaker for 90 min at room temperature (25 °C). The washed residue was separated from the solution by vacuum filtration and dried overnight in an oven. The dried washed residue is shown in Figure 2b and is found to be more amenable to characterization than the raw residue.

2.3.1. Specific Gravity

The measured specific gravity (Gas pycnometer, HumiPyc model 2 from Instruquest, Coconut Creek, FL, USA) of the washed ZPR is 3.95 g/cm3. Since the densities of zinc and of the cemented metals are all above 5 g/cm3 this result indicates that the residue is not made exclusively of pure metals.

2.3.2. Size Distribution

Figure 3 shows the particle size distribution obtained by sieving the washed ZPR on a Tyler screen series from 1.2 mm down to 0.038 mm. The ZPR is coarse with a D80 of about 900 µm. The material coarseness will pose a problem for the sampling for assaying of the residue. Indeed, since assaying of the sample implies collecting a 0.5–1.0 g sample for the digestion prior to analysis using the emission spectrometer (Section 2.1), one can expect a significant variability in the assays of the residue due to the fundamental error of sampling [12]. For ore type material, this error is reduced by pulverizing the sample prior to sampling. However, the metallic and ductile nature of the ZPR makes impossible the pulverization of the sample, and thus one should expect a variability in the assays that data reconciliation [13,14,15,16] as applied here should be able to attenuate.

2.3.3. Chemical Composition

Table 2 gives the chemical composition of the ZPR sample. The measured assays of the sample are compared (see Table 2) to the typical composition of the ZPR provided by the CEZinc plant. The general proximity of the sample composition with the typical composition of the residue provided by CEZinc confirms that the received sample is representative of the residue usually released by the plant. The difference in the composition is attributed to the washing as discussed later. The Co content is consistent with typical ZPR from other zinc smelters [1,2,3].

2.3.4. X-ray Diffraction (XRD)

Figure 4 shows the XRD pattern (Instrument: Aeris, Malvern Panalytical (Malvern, UK) obtained for the residue. The XRD shows the presence of metallic zinc, copper, and possibly metallic lead. The peaks for Cd and Co are not visible due to the low contents of these elements. The presence of Pb is confirmed by the assays (see Table 2) and is reported under the form of PbO2 for the residue of an Iranian zinc smelter [3] and under the form of PbSO4 [10] for a Chinese zinc residue. The XRD results of Figure 4 also show the presence of copper, zinc, and calcium sulfates likely responsible for the observed low specific gravity of the residue (Section 2.3.1). These sulfates, except gypsum, could be completely removed by a longer or slightly acidic or hot water wash of the residue as reported in [2].

3. Results

3.1. Washing of the ZPR

The first step of the proposed process is the washing of the ZPR. Initially done to eliminate the sulfuric acid from the ZPR, the washing step provides an economic way to pre-concentrate the cobalt by allowing a partial elimination of the soluble zinc and cadmium sulfates contained in the ZPR. The results of a washing test are shown in Figure 5 and Table 3. Washing is carried out at room temperature using water at 15% solids in mass. Figure 5 shows the measured concentrations of Zn, Cd, Ca, Co, and Cu during washing. The solution pH falls from 7.2 to 6.3 during the washing step due to the release of the residual sulfuric acid. Table 3 gives the proportions of metals removed from the ZPR calculated using:
D m = 100 V x m V x m + W ZPR y ZPR
where Dm is the dissolved proportion of metal m, V is the volume (L) of the wash solution, xm the metal content (g/L) in the solution. WZPR and y Z P R are, respectively, the weight (g) and the fraction of metal m in the dried washed ZPR. Results presented in Table 3 show that, respectively, 20% and 43% of the zinc and cadmium contained in the raw ZPR are removed by a 30 min wash. About 4% of the cobalt contained in the ZPR is lost during the operation. Higher impurity removal can be achieved by washing the ZPR for 90 min but at increased cobalt losses as shown in Figure 5. The zinc is likely under an insoluble metallic form as metallic zinc dust is used for the cementation, while cadmium is likely present as a sulfate. The 4% Co dissolution is an indication that some cobalt is under the form of sulfate, with the remaining being metallic. The washing step can be viewed as a selective leaching operation for which the leaching conditions are adjusted to target specific metals [1,2]. The use of diluted acid in replacement of water could yield a better elimination of zinc and cadmium at the expenses of more important cobalt losses into the wash solution [10].

3.2. Preparation of ZPR Samples for the Co Extraction Tests

The leaching tests are carried out using samples prepared by washing 75 g of raw ZPR for 30 min using the above described approach. The washed material is dried at low temperature in an oven. The use of 75 g batches was found to be a good compromise between the variability of the 75 g batch composition [17] and the mass of material to be manipulated during the experimentation. Table 4 gives the assays obtained by assaying three (3) randomly selected 75 g batches.

3.3. Leaching of the Washed ZPR

The next step of the process is to leach the metals out of the ZPR into an aqueous solution from whichi it will be possible to separate the cobalt from the other metals. The leaching tests are conducted in a mechanically agitated beaker for 30 min using a weight L/S ratio of 15/1 at 80 °C. Leaching tests are carried out with sulfuric acid as it is the acid used in the zinc plant that provided the ZPR. Table 5 gives the average proportion of metals dissolved (±standard deviation) of three (3) leaching tests and the average metal contents in the liquor. About 65% of the solids in the ZPR are dissolved during the leaching process with 98% of the cobalt effectively leached off the ZPR, a performance similar to that reported in [10].

3.4. Selective Precipitation of the Cobalt from the Pregnant Liquor Solution

The main impurities in the pregnant liquor solution are Zn, Cd, Ni, Fe, and Cu (Table 5). The approach used to selectively separate cobalt from these elements begins with an oxidation of iron and manganese to precipitate of these oxidized elements by increasing the pH near 3.0 while Cu, Zn, Cd, and Co(II) remain in the solution. The next step is to oxidize Co(II) to Co(III) and to precipitate Co(III) by increasing the pH above 3.0 leaving Zn, Cd, Ni and Cu in the solution.
Ammonium PerSulfate or APS ((NH4)2S2O8), as discussed in [1,8], provides the required oxidation potential for iron, manganese and subsequently cobalt. The sequence of the steps followed to precipitate the cobalt is shown in Figure 6.

3.4.1. Precipitation of Fe-Mn

Sodium hydroxide is firstly added to the pregnant liquor solution to bring the pH to 3.0. APS is then added to the solution to increase the Redox potential from 90 to 650 mV. During the oxidation process, the pH of the solution is maintained at 3.0 by a regular addition of NaOH. Samples of the solution were collected at different Eh values and analyzed for Fe, Mn, and Co. As anticipated [1] Fe and Mn precipitate prior to Co a behavior confirmed by the variations of the metal contents in the solution as shown in Figure 7. According to Figure 7, the optimal Eh for the precipitation of Fe and Mn without precipitation of Co is 650 mV and the minimum Eh for the precipitation of Co is 1000 mV. These Eh values are coherent with those reported in [1]. Table 6 gives the proportions of the metals in the leached solution that are removed by the oxidation to 650 mV. Iron and manganese are almost completely removed from the solution. Ideally, cobalt should not be precipitated at this stage; however, it was observed that a close control of the Eh was not always possible as the Redox probe shows a significant measurement variability causing cobalt losses (~17%) in the Fe–Mn precipitate. The difficulty in the control of the Eh is attributed to the probe and to its sensitivity to the APS addition. Indeed, a small addition of APS can make a large local step in the Redox potential of the solution. It is likely that a process solely based on the use of an APS dosage [1,8] is not recommended to achieve a selective separation. Cleary the oxidant addition should be based on a reliable measurement of the ReDox potential of the solution and not on the dosage of the oxidant.
Once the Redox potential reaches 650 mV, the addition of APS is stopped and the iron and manganese precipitate are removed by filtration (see Figure 6). The filtration of the sludgy Fe-Mn precipitate is difficult and is believed to be one of the reasons for the loss of cobalt at this stage. Ensuring a rapid and adequate filtration of the solution after the end of the reaction seems critical to limit cobalt losses. The solution from that solid/liquid separation advances to the cobalt precipitation step (Figure 6). Results of Table 6 show that Mn and Fe are effectively removed from the solution at the expenses of some cobalt losses. The large standard deviation observed for the fraction of cobalt precipitated is attributed to Eh measurement problems as discussed above and difficulties in the filtration of the precipitate from one test to another one. Improving on the accuracy of the Eh measurement method and of the solids/liquid separation of the Fe–Mn precipitate could significantly improve the global recovery of cobalt.

3.4.2. Precipitation of Co

The cobalt precipitation is carried out by adding APS to bring the Redox to 1000 mV and keeping the solution at 80 °C to accelerate the precipitation [1]. The precipitation of cobalt under the form of CoOOH is slow as shown in Figure 8a. This observed behavior is consistent with previously reported results [1] reproduced in Figure 8b. Table 7 gives the variation of the solution composition from the leach step to the Co precipitation one. Zn, Cd, and Cu remain in the solution while cobalt precipitates with some of the iron and manganese remaining in the solution after the first oxidation step. Table 8 gives the proportions of the different metals precipitated during the cobalt precipitation step. About 2% of the copper precipitates with the cobalt and represents a critical impurity as discussed later. The fact that the observed Co precipitation rate in Figure 8 is significantly less than that reported in [1] is an indication that there is room to improve the proposed processing scheme in order to reduce the precipitation time and subsequently the volume of the precipitation vessels for a continuous process.

3.4.3. Washing and Composition of the Cobalt Precipitate

The cobalt precipitate is washed with water at 80 °C at 1% solids for 5 min, filtered, dried overnight, weighed, and assayed. Table 9 gives the composition of the cobalt product obtained from 3 independent tests. Table 9 compares the average composition of the cobalt product to a target cobalt hydroxide feed for a cobalt refinery [18]. Results show that some tunings (likely at the cobalt precipitation stage) of the process are still required to lower the zinc and copper contents to meet the composition of the feed material for the Co-refinery.
The XRD powder pattern of the cobalt product is shown in Figure 9. Results confirm that the produced material is under the form of CoO(OH) and Co(OH)2. The presence of these compounds was expected based on observations from other researchers [1].

3.5. Overall Process Performance and Quality of the Product

The process flow sheet for the extraction of cobalt from the ZPR is shown in Figure 10. The flowsheet has similarities with the flowsheet presented in [1]. The similarity between the two flowsheets developed independently is an indication that this processing scheme is a viable route for the recovery of cobalt from a ZPR produced by cementation on zinc dust.
In order to assess the robustness of the proposed process, the whole processing sequence of Figure 10 was repeated with three ZPR feed samples. The previous sections gave the results of the repetitions obtained for the various stages of the process. Table 10 summarizes these results in terms of cobalt distribution. The repetitions show that the critical step in the proposed process is the oxidation/precipitation of the iron and manganese prior to the cobalt precipitation. The main cobalt losses occur at the Fe-Mn precipitation step. A problem or inaccuracy in the measurement of the Redox potential and the difficulties in the filtration of the Fe-Mn sludge cause some Co precipitation and an incomplete removal of impurities that will subsequently contaminate the cobalt product. Cobalt losses also occur at the final precipitation step, where recovery could be improved by using a pH above 3.0 and allowing more time for precipitation [1]. However, the use of a higher pH and of an increase precipitation time may cause more impurities to precipitate with the cobalt. This optimization problem of maximizing Co recovery under the constraint of an acceptable product purity can be adequately tackled down using a factorial Design Of Experiments (DOE) [19] if the process is to be continued with an optimization phase. The aspect of the process sensitivity to operating conditions, particularly the control of the Redox potential, addressed here is seldom discussed in the literature dealing with the recovery of cobalt from a ZPR, while it is as important as the process itself, especially if it is to go on to piloting.
In summary, the proposed processing flow sheet yields a Co product assaying 45 ± 4% Co at a recovery of 62%. Improvements to the reproducibility of the method can be achieved by improving the control of the Redox potential and the solids/liquid separation of the precipitated Fe-Mn sludge. These results cannot be compared to those of other processes used for processing a ZPR produced by cementation on zinc dust, as it was not possible to find such data in the literature.
Ideally, to avoid paying refining charges from the selling of the cobalt hydroxide product to a custom Co refinery, one should aim at producing electrolysis-grade cobalt at the end of the ZPR-Co process. The concentration of cobalt in the solution released by the S/L separation of the Fe-Mn precipitate is low at 3 g/L, and should be increased to at least 45 g/L [20] to allow Co electro-winning. Solvent Extraction (SX) is an approach to increase the solution concentration and remove some of the accompanying impurities (See Table 9). The other option is to stock pile the produced Co hydroxide and to dissolve it under reducing conditions to convert Co(III) into Co(II) with a controlled amount of sulfuric acid to generate the solution to feed the electrolytic cells. Figure 11 shows the two options.

3.6. Economics of the Process

The analysis presented in this section focuses only on the operating costs of the process of Figure 10. It is a preliminary analysis and the calculated costs should be considered as Class 5 estimates (AACE International). Results are used to anticipate the economic viability of the process and decide on the continuation of the laboratory test work to optimize the proposed ZPR-Co process.
A cobalt price of 30.20 USD/kg (LME Price August 2020) is used to estimate the revenues that can be generated by processing the ZPR. The Net Smelter Return, if the cobalt hydroxide is to be sold to a refinery, is estimated by assuming that 90% of the cobalt in the hydroxide is payable and that the refining charges are 3.00 CAD/kg of Cobalt hydroxide. If the cobalt content of the produced Co hydroxide is 45% (see Table 9) then the revenues (assuming an exchange rate of 1.25 CAD/USD) generated per kg of cobalt hydroxide are:
N S R = 0.9 × 0.45 × 30.2 × 1.25 3 = 12.28   CAD $ kg   of   Co   hydroxide ,
Since the test work has shown that the processing of 75 g of ZPR yields 1.2 g of Co hydroxide, the potential revenues per kg of ZPR are 0.20 CAD/kg ZPR.
The operating costs considered here are due to the reagents and exclude the energy costs for heating the solution at the precipitation stage. Table 11 gives the calculated operating costs per kg of ZPR. The reagent costs are probably over-estimated as purchasing the sulfuric acid may not be required. Indeed some spent zinc electrolyte could be used for the Co process (see Figure 1). Additionally, it is very likely that recycling some of the solution streams of the ZPR-Co process could allow a reduction in the consumption of caustic and APS. This preliminary evaluation shows that the proposed process is not viable but the process certainly deserves to be optimized to increase the overall cobalt recovery and to reduce the consumption of APS that is the main contributor to the operating costs. The option of producing metallic cobalt rather than cobalt hydroxide should also be investigated.

3.7. Residues of the ZPR-Co Process

The proposed process generates two solid residues (the ZPR leached residue, the Fe–Mn precipitate) and two liquid effluents (the solutions from the ZPR washing and from the Co precipitation as indicated in Figure 12. Table 12 gives the compositions of the liquid and solid residues. The copper content of the ZPR leached solids is 36%, which is above the copper content of the ZPR (see Table 2). If the metals of the reject solutions were to be precipitated under the form of hydroxides by increasing the pH above 9.0, the precipitate would assay 13% Cu, which is still in the range of the ZPR copper content. Thus, two of the residues of the ZPR-Co process could possibly be used as copper sources and possibly be sold to a Cu smelter.

4. Conclusions

A process to obtain a cobalt rich hydroxide from the processing of a Cu–Cd–Co residue produced by cementation on zinc dust is described in this paper. The process includes a water leaching of the residue to remove soluble Zn and Cd. The washed residue is leached for 30 min with sulfuric acid (100 g/L) at a pH of 0.2. The Fe and Mn of the leach solution are precipitated by increasing the Eh to 650 mV while maintaining a pH of 3.0 with sodium hydroxide. Cobalt hydroxide is finally precipitated by increasing the Eh to 1000 mV. Repetition of the whole processing flow sheet shows that the critical steps of the process are the control of the Eh at the precipitation stage and the solids/liquid filtration of the Fe–Mn precipitate. The cobalt recovery from the zinc residues to the cobalt hydroxide is 62 ± 14%. The cobalt content of the cobalt product is 45 ± 4%. The variability in the results is mainly due to the control and measurement of the solution Redox potential

Author Contributions

Conceptualization, investigation, formal analysis methodology, data curation, writing—review and editing, L.B.; conceptualization, investigation, formal analysis methodology, data curation, supervision, writing—review and editing, K.T. and J.-F.B.; writing—original draft preparation, writing—review and editing, formal analysis, supervision, project administration, C.B.; funding acquisition, conceptualization, review, G.H. All authors have read and agreed to the published version of the manuscript.

Funding

This research was funded by Institut de recherche de Hydro-Québec.

Acknowledgments

The authors acknowledge the financial support of the Institut de recherche de Hydro-Québec and CEZinc for providing the zinc residues sample for the testwork. E. Benguerel, of CEZinc, is also acknowledged for reviewing the paper prior to publication.

Conflicts of Interest

The authors declare no conflict of interest.

References

  1. Huang, Y.; Zhang, Z.; Cao, Y.; Han, G.; Peng, W.; Zhu, X.; Zhang, T.-A.; Dou, Z. Overview of cobalt resources and comprehensive analysis of cobalt recovery from zinc plant purification residue-a review. Hydrometallurgy 2020, 193, 3–12. [Google Scholar] [CrossRef]
  2. Wang, Y.; Zhou, C. Hydrometallurgical process for recovery of cobalt from zinc plant residue. Hydrometallurgy 2002, 63, 225–234. [Google Scholar] [CrossRef]
  3. Fattahi, A.; Rashchi, F.; Abkhoshk, E. Reductive leaching of zinc, cobalt and manganese from zinc plant residue. Hydrometallurgy 2016, 161, 185–192. [Google Scholar] [CrossRef]
  4. Anonymous. Critical Materials Rare Earths Supply Chain: A Situational White Paper; U.S. Department of energy, Office of Energy Efficiency & Renewable Energy: Washington, DC, USA, 2020.
  5. Golmohammadzadeh, R.; Faraji, F.; Rashchi, F. Recovery of lithium and cobalt from spent lithium ion batteries (LIBs) using organic acids as leaching reagents: A review. Resour. Conserv. Recycl. 2018, 136, 418–435. [Google Scholar] [CrossRef]
  6. Frankel, T.C. The Cobalt Pipeline: Tracing the Path from Deadly Hand-Dug Mines in Congo to Consumer’s Phones and Laptops. The Washington Post. 1 October 2016. Available online: https://longform.org/posts/the-cobalt-pipeline (accessed on 3 November 2020).
  7. Ashtari, P.; Pourghahramani, P. Hydrometallurgical recycling of cobalt from zinc plants residue. J. Mater. Cycles Waste Manag. 2018, 20, 155–166. [Google Scholar] [CrossRef]
  8. Güler, E.; Seyrankaya, A. Precipitation of impurity ions from zinc leach solutions with high iron contents—A special emphasis on cobalt precipitation. Hydrometallurgy 2016, 164, 118–124. [Google Scholar] [CrossRef]
  9. Bøckman, O.; Østvold, T. Products formed during cobalt cementation on zinc in zinc sulfate electrolytes. Hydrometallurgy 2000, 54, 65–78. [Google Scholar] [CrossRef]
  10. Qian, L.; Zhang, B.; Min, X.-B.; Shen, W.-Q. Acid leaching kinetics of zinc plant purification residue. Trans. Nonferrous Met. Soc. China 2013, 23, 2786–2791. [Google Scholar]
  11. CEzince Company. Available online: https://www.cezinc.com/fr/Pages/home.aspx (accessed on 5 August 2020).
  12. Gy, P.M. Sampling of Particulate Materials, Theory and Practice; Elsevier: Amsterdam, The Netherlands, 1982. [Google Scholar]
  13. Bazin, C.; Hodouin, D.; Zouadi, M. Data reconciliation and equilibrium constant estimation: Application to copper solvent extraction. Hydrometallurgy 2005, 80, 43–53. [Google Scholar] [CrossRef]
  14. Hodouin, D.; Everell, M. A hierarchical procedure for adjustment and material balancing of mineral processes data. Int. J. Miner. Process. 1980, 7, 91–116. [Google Scholar] [CrossRef]
  15. Hodouin, D.; Flament, F.; Bazin, C. Reliability of material balance calculations a sensitivity approach. Miner. Eng. 1989, 2, 157–169. [Google Scholar] [CrossRef]
  16. Turgeon, K.; Bazin, C.; Boulanger, J.-F.; Whitty-Léveillé, L.; Larivière, D. Material balancing and estimation of equilibrium constants: Application to solvent extraction tests of rare earth elements. In Proceedings of the International Mineral Processing Congress, Quebec, QC, Canada, 11–15 September 2016. [Google Scholar]
  17. Bazin, C.; Hodouin, D.; Blondin, R.M. Estimation of the variance of the fundamental error associated to the sampling of low grade ores. Int. J. Miner. Process. 2013, 124, 117–123. [Google Scholar] [CrossRef]
  18. Zhan, D.; Marquez, J. First Cobalt Corporation: 2019 First Cobalt Refinery Restart. 103870-RPT-0001. Available online: https://www.firstcobalt.com/_resources/reports/20190627-Ausenco-ConceptualStudy_Rev-E.pdf (accessed on 20 November 2020).
  19. Box, G.E.; Draper, N.R. Evolutionary Operation: A Statistical Method for Process Improvement; Wiley: New York, NY, USA, 1969; Volume 25. [Google Scholar]
  20. Conard, B. History of electrolytic cobalt refining at Vale Canada (Inco). CIM J. 2015, 6, 51–58. [Google Scholar] [CrossRef]
Figure 1. Simplified flowsheet of the zinc extraction process.
Figure 1. Simplified flowsheet of the zinc extraction process.
Metals 10 01553 g001
Figure 2. ZPR as is and after washing with water. (a) Raw residue after drying; (b) Residue after washing and drying.
Figure 2. ZPR as is and after washing with water. (a) Raw residue after drying; (b) Residue after washing and drying.
Metals 10 01553 g002
Figure 3. Size distribution of the residue.
Figure 3. Size distribution of the residue.
Metals 10 01553 g003
Figure 4. XRD powder pattern of the CEZinc ZPR.
Figure 4. XRD powder pattern of the CEZinc ZPR.
Metals 10 01553 g004
Figure 5. Dissolved proportion of metals in time (25 °C, 15% solids in mass).
Figure 5. Dissolved proportion of metals in time (25 °C, 15% solids in mass).
Metals 10 01553 g005
Figure 6. Process for the extraction of cobalt from the ZPR.
Figure 6. Process for the extraction of cobalt from the ZPR.
Metals 10 01553 g006
Figure 7. Precipitation of Fe and Mn with increasing the Eh while maintaining a pH of 3.0 (a) Fe, Mn, and Co contents in the solution during the oxidation to 1000 mV. (b) Fe and Mn contents in the solution during the oxidation below 1000 mV.
Figure 7. Precipitation of Fe and Mn with increasing the Eh while maintaining a pH of 3.0 (a) Fe, Mn, and Co contents in the solution during the oxidation to 1000 mV. (b) Fe and Mn contents in the solution during the oxidation below 1000 mV.
Metals 10 01553 g007
Figure 8. Cobalt precipitation rates. (a) Observed rate of Co precipitation (pH = 3.0, Eh = 1000 mV, 80 °C, 1 g/L Co). (b) Rates of Co precipitation reported in [1] B-0.
Figure 8. Cobalt precipitation rates. (a) Observed rate of Co precipitation (pH = 3.0, Eh = 1000 mV, 80 °C, 1 g/L Co). (b) Rates of Co precipitation reported in [1] B-0.
Metals 10 01553 g008
Figure 9. XRD powder pattern of the cobalt product.
Figure 9. XRD powder pattern of the cobalt product.
Metals 10 01553 g009
Figure 10. ZPR processing circuit to extract cobalt (See Table 10 for the composition of streams 1–6).
Figure 10. ZPR processing circuit to extract cobalt (See Table 10 for the composition of streams 1–6).
Metals 10 01553 g010
Figure 11. Processing options to produce electrolytic cobalt.
Figure 11. Processing options to produce electrolytic cobalt.
Metals 10 01553 g011
Figure 12. Liquid and solid residues generated by the ZPR-Co process.
Figure 12. Liquid and solid residues generated by the ZPR-Co process.
Metals 10 01553 g012
Table 1. Reagents used for the experimentation.
Table 1. Reagents used for the experimentation.
ReagentCompositionBrand and Purity
Sulfuric acidH2SO4Fisher, 98% purity
Sodium hydroxideNaOHFisher, 98.8% purity
Ammonium persulfate(NH4)2S2O8Alfa Aesar, 98% purity
Table 2. Composition of the ZPR.
Table 2. Composition of the ZPR.
ElementsCEZ Typical CompositionSample Composition *
%%
Zn20–2516.0±0.5
Cd2–63.5±0.2
S-5.7±0.8
Cu15–2511.9±0.4
Ca-0.76±0.04
Co2–41.7±0.1
Ni0–20.44±0.04
Fe0–10.34±0.02
Mn-0.22±0.01
Pb9–124.0±0.1
*: Average ± standard deviation of three samples.
Table 3. Dissolved metals after 30 min of washing with water (25 °C, 15% solids in mass).
Table 3. Dissolved metals after 30 min of washing with water (25 °C, 15% solids in mass).
Metal% Dissolved *
Zn20±3
Cd43±2
Cu0.03±0.02
Ca16±1
Co4±1
Ni2±1
Fe0.4±0.2
Mn84±3
Pb0.1±0.2
*: average ± standard deviation of three tests.
Table 4. Chemical assays (%) of three randomly selected feed samples (Smp = Sample; Avg = Average; Std-dev =Standard deviation RSD: = Std-Dev/Avg).
Table 4. Chemical assays (%) of three randomly selected feed samples (Smp = Sample; Avg = Average; Std-dev =Standard deviation RSD: = Std-Dev/Avg).
ElementsSmp #1Smp #2Smp #3AvgStd-DevRSD (%)
Zn16.416.215.516.00.53
Cd3.73.53.33.50.26
Cu11.512.112.211.90.43
Ca0.800.770.720.760.045
Co1.681.801.631.710.095
Ni0.470.470.400.440.049
Fe0.360.340.310.340.026
Mn0.230.210.230.220.015
Pb3.84.14.04.00.13
Table 5. Proportion of the metals dissolved during the leaching of the ZPR (Average (±standard deviation) of the results of three (3) leaching tests and the average composition of the liquor (Ratio L/S: 15/1; 100 g/L H2SO4, Eh = 90 mV, pH = 0.2, 30 min, 80 °C).
Table 5. Proportion of the metals dissolved during the leaching of the ZPR (Average (±standard deviation) of the results of three (3) leaching tests and the average composition of the liquor (Ratio L/S: 15/1; 100 g/L H2SO4, Eh = 90 mV, pH = 0.2, 30 min, 80 °C).
Species% DissolvedLiquor Concentration (mg/L)
Solids65±1
Zn97.1±0.411,800
Cd91±2370
Cu37±33600
Ca88±3252
Co97±11170
Ni97±1345
Fe98±2270
Mn91±1626
Pb0.2±0.36
Table 6. Metal precipitation during the oxidation for Fe-Mn removal of the leach solution (Average (±standard deviation) results of three (3) tests (Eh = 90 to 650 mV, pH = 3.0, 80 °C, 15 min).
Table 6. Metal precipitation during the oxidation for Fe-Mn removal of the leach solution (Average (±standard deviation) results of three (3) tests (Eh = 90 to 650 mV, pH = 3.0, 80 °C, 15 min).
Species% Precipitated
Zn0.3±0.2
Cd0.6±0.2
Cu1.1±0.4
Ca1.1±0.6
Co17±8
Ni0.6±0.3
Fe80±20
Mn90±10
Table 7. Composition of the solutions from the ZPR leach, Fe-Mn and Co precipitation steps.
Table 7. Composition of the solutions from the ZPR leach, Fe-Mn and Co precipitation steps.
All Concentrations in mg/L
SolutionVolume (mL)ZnCdCuCoFeMn
Leach solution84111,8003703600117027026
After Fe-Mn ppt94410,5113273200860461.3
After Co ppt97510,111318300084160.4
Table 8. Metal precipitation during the cobalt precipitation stage (Average ± standard deviation) for three (3) tests (Eh = 1000 mV, pH = 3.0, 80 °C, 120 min).
Table 8. Metal precipitation during the cobalt precipitation stage (Average ± standard deviation) for three (3) tests (Eh = 1000 mV, pH = 3.0, 80 °C, 120 min).
Species% Precipitated
Zn0.4±0.1
Cd1±0.3
Cu2±1
Ca1±0.4
Co89±3
Table 9. Composition (%) of the produced cobalt hydroxide and specifications for the feed of a custom cobalt refinery.
Table 9. Composition (%) of the produced cobalt hydroxide and specifications for the feed of a custom cobalt refinery.
MaterialCoCdCuZnFeMnNiPb
Produced Co hydroxide *45 ± 40.120 ± 0.0044.4 ± 0.70.8 ± 0.22 ± 1<0.1<0.10.3 ± 0.1
Custom refinery Co hydroxide feed [19]23.2n.a.1.610.192.393.270.39n.a.
*: Average ± standard deviation of three (3) replicated tests.
Table 10. Distribution (%) of the cobalt in the process streams of the circuit of Figure 9.
Table 10. Distribution (%) of the cobalt in the process streams of the circuit of Figure 9.
Process StreamStream Number as in Figure 10Avg.Std-Dev
ZPR1100100
Washed solids ZPR2863
Leach solution3844
Co ppt feed solution47010
Spent solution from Co ppt571
Cobalt hydroxide66214
Table 11. Preliminary estimation of the operating costs for the ZPR-Co process of Figure 9. (The reagent prices were obtained from quotations dating of 2019 and are used here only to give an order of magnitude).
Table 11. Preliminary estimation of the operating costs for the ZPR-Co process of Figure 9. (The reagent prices were obtained from quotations dating of 2019 and are used here only to give an order of magnitude).
ReagentConsumption (kg/kg of ZPR)Price CAD$/kgCAD$/kg ZPR
H2SO41.90.1700.032
NaOH0.070.800.056
APS0.250.850.22
Total costs--0.30
Gross revenues--0.20
Benefits (losses)--(0.10)
Table 12. Metal contents in the residues of the ZPR-Co process.
Table 12. Metal contents in the residues of the ZPR-Co process.
Residues from the ZPR-Co ProcessContent (mg/L or %)
ZnCdCu
Soln from washing (mg/L)120230673.6
Soln from Co ppt (mg/L)11113173028
Leach solid residue (%)2.060.2236.4
Fe-Mn solid residue (%)2.090.131.97
Publisher’s Note: MDPI stays neutral with regard to jurisdictional claims in published maps and institutional affiliations.

Share and Cite

MDPI and ACS Style

Boisvert, L.; Turgeon, K.; Boulanger, J.-F.; Bazin, C.; Houlachi, G. Recovery of Cobalt from the Residues of an Industrial Zinc Refinery. Metals 2020, 10, 1553. https://doi.org/10.3390/met10111553

AMA Style

Boisvert L, Turgeon K, Boulanger J-F, Bazin C, Houlachi G. Recovery of Cobalt from the Residues of an Industrial Zinc Refinery. Metals. 2020; 10(11):1553. https://doi.org/10.3390/met10111553

Chicago/Turabian Style

Boisvert, Laurence, Keven Turgeon, Jean-François Boulanger, Claude Bazin, and Georges Houlachi. 2020. "Recovery of Cobalt from the Residues of an Industrial Zinc Refinery" Metals 10, no. 11: 1553. https://doi.org/10.3390/met10111553

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.

Article Metrics

Back to TopTop