Next Article in Journal
Experimental and Computational Study of Microhardness Evolution in the HAZ for Al–Cu–Li Alloys
Next Article in Special Issue
Structural Evolution and Mechanical Behavior of Ytterbia Doped Hafnia Biphasic Ceramics under Annealing at 1500 °C
Previous Article in Journal
Crystalline Microstructure, Microsegregations, and Mechanical Properties of Inconel 718 Alloy Samples Processed in Electromagnetic Levitation Facility
Previous Article in Special Issue
Effect of TiO2 on the Microstructure and Flexural Strength of Lunar Regolith Simulant
 
 
Font Type:
Arial Georgia Verdana
Font Size:
Aa Aa Aa
Line Spacing:
Column Width:
Background:
Article

Rapid Growth of Niobium Oxide Nanowires by Joule Resistive Heating

by
Aarón Calvo-Villoslada
,
Paloma Fernández
and
Belén Sotillo
*
Department of Materials Physics, Faculty of Physics, Complutense University of Madrid, 28040 Madrid, Spain
*
Author to whom correspondence should be addressed.
Crystals 2024, 14(3), 245; https://doi.org/10.3390/cryst14030245
Submission received: 16 February 2024 / Revised: 24 February 2024 / Accepted: 27 February 2024 / Published: 1 March 2024
(This article belongs to the Special Issue Ceramics: Processes, Microstructures, and Properties)

Abstract

:
Joule heating of niobium (Nb) metal wires by running a high electric current density through them has been used to grow Nb2O5 nanowires. The formation of a micrometric oxide layer on the Nb wires has also been observed. The size and density of the nanowires are related to the current values applied, as well as the thickness of the oxide layer formed. Characterization of both nanowires and oxide layer has been performed using X-ray diffraction, scanning electron microscopy, energy dispersive X-ray microanalysis, and micro-Raman spectroscopy. It has been observed that this method allows the growth of Nb2O5 nanowires in times as short as tens of seconds.

1. Introduction

Transition metal oxides (TMOs) constitute a class of materials that possesses unique electronic, magnetic, and optical properties, making them attractive for a wide range of applications, including catalysis, energy storage, and electronic devices [1,2,3,4]. Among the different TMOs, niobium oxides are attractive candidates for these applications due to their hardness and resistance to corrosion, chemical stability, and non-toxicity. However, niobium oxides may present a huge diversity of compositions and crystal structures, which hinders the development of a complete description relating the phases of these oxides with their physico-chemical properties. Despite this, it is worthwhile to increase our comprehension of niobium oxides, as they are materials that withstand aggressive environments well and could therefore increase the useful life of different devices, such as sensors or energy storage devices.
Among the different oxides that niobium can form, niobium pentoxide is the most stable one, in which Nb has an oxidation state of +5 (Nb2O5). Nb2O5 may have different crystal structures depending on the treatment applied to the material [5]. The most frequently observed ones are the pseudo-hexagonal phase (TT-Nb2O5), which appears when Nb metal, NbO, NbO2, or amorphous oxides are heated between 320 and 350 °C in air; the orthorhombic phase (T-Nb2O5), which is obtained when Nb metal, NbO, NbO2, amorphous oxide, or TT-Nb2O5 are heated between 600 and 800 °C; and the monoclinic phase (H-Nb2O5). H-Nb2O5 is the most stable phase once formed, and it always appears when the oxide is treated at high temperatures in air (>900 °C).
To obtain Nb2O5 nanostructures, several methods have been employed [6]. The most common ones are hydrothermal synthesis [7,8] and sol-gel synthesis [9,10]. With these methods, a wide range of structures with different shapes and dimensionality can be obtained. In general, low temperatures are used (in the range of 100–200 °C, although in some cases a post-treatment at higher temperatures is required [6]) and synthesis times of hours to days. On the other hand, thermal heating of Nb metal foils has also been used to obtain a high density of nanowires [11,12,13]. The growth conditions of this last method would be more comparable with the experiments performed in this work. In general, the thermal treatment of Nb2O5 oxide powders only produces structures in the micrometric range [14]. For all these growth strategies, the time required is in the range of hours. For example, in the case of thermal heating of Nb metal foils, times range from 1 h up to 6 h, temperatures are above 800 °C (generally 900 °C), and the treatment must be performed in a low-oxidizing atmosphere (low vacuum or Ar flux). Rapid growth of Nb2O5 nanowires by cold oxygen plasma treatment of Nb foils has been reported [15], with a growing time of 90 s in vacuum.
In this work, Nb2O5 nanowires and micrometric oxide layers have been obtained by Joule resistive heating of Nb metal wires in air. This strategy has been successfully applied for the rapid growth of oxide nanowires of Zn, Cu, W, Mo, or V [16,17,18,19,20], and core-shell metal-oxide structures [21,22]. However, to the best of our knowledge, this rapid growth has not yet been studied in detail in Nb metal wires. The rapid growth observed in these studies is associated with a diffusion process of the oxygen inside the metal that is accelerated by electromigration due to the high electrical currents employed [23]. Nb2O5 material obtained with this technique can be applied where having the oxide on a metallic substrate is useful, such as in energy storage devices [24,25], sensing devices [12], or field emitters [11].

2. Materials and Methods

The starting material is a niobium metal wire purchased from Thermo Scientific (Waltham, MA, USA) (purity 99.99% metal basis excluding Ta) with a diameter of 0.25 mm. Segments of 7 cm in length are cut and mounted on the homemade platform used to grow the oxide nanowires (Figure 1a). As can be seen in the figure, the Nb metal wire is contacted on two steel electrodes, leaving a wire distance of 5 cm suspended in air. The electrodes are contacted to the current source (EA-PS 3016-40 B), which can supply currents up to 40 A (max. power of 640 W). To study the growth conditions, current value and growth time are varied. The voltage variation observed during the treatment is also measured. The final selected growth parameters are shown in Table 1.
As a consequence of Joule heating, a temperature gradient is established along the metallic wire [20,22]. The increase in temperature promotes the formation of oxide nanowires and a micrometric oxide shell covering the original metallic wire. The maximum temperature (Table 1) is achieved at the center of the length of the Nb wire, while it decreases as we approach the electrodes (Figure 1b), i.e., electrodes are acting as heat drains. The maximum temperature reached is measured using an optical pyrometer Infratherm IGA 12-S calibrated with the emissivity of Nb. The current value is fixed in the current source before starting the growing process, so that value is applied to the Nb wire instantly, giving a rate of temperature increase of about 500 °C/s.
Electrical characterization of the Nb metal wire is performed using a Keithley 2400 Series SourceMeter (Cleveland, OH, USA). Meanwhile, the oxide formed is characterized by means of X-ray diffraction (XRD), scanning electron microscopy (SEM), energy dispersive X-ray microanalysis (EDX) and micro-Raman spectroscopy (µ-RS), in order to assess their composition and crystal structure. All the measurements are done at room temperature. Cross-section of the Nb metal wires is carried out by embedding the wires in a commercial resin and cutting them with a diamond saw.
XRD measurements are done in a PANalytical X’Pert Powder diffractometer (X-ray diffraction CAI Centers of UCM) in the Bragg–Brentano geometry using Cu–Kα radiation, with a step in 2θ of 0.05°. The morphology of the obtained oxide is studied using a FEI Inspect-S SEM (FEI Company, Eindhoven, Netherlands) working at 20 kV. Additional optical microscope images are recorded with a Leica DFC295 digital camera mounted on a Leica MSV266 microscope (Leica Microsystem, Wetzlar, Germany). For EDX measurements, a Bruker QUANTAX 70 detector (Bruker, Berlin, Germany) attached to a Hitachi TM3000 (Hitachi High Technologies Corporation, Tokyo, Japan) working at 15 kV is employed. The EDX data are analyzed using Bruker ESPRIT QUANTAX 70 EDS software.
µ-RS measurements are carried out with a confocal microscope Horiba JobinYvon LABRAM-HR (Horiba JobinYvon, Villeneuve d’Ascq, France), using the 632.8 nm line of a He–Ne laser. The laser is focused onto the sample using a 100× Olympus objective (0.9 NA), and the scattered light is collected using the same objective (backscattering configuration). The grating employed to analyze the signal has 600 L/mm, and afterwards the signal is recorded with an air-cooled charge-coupled device camera (CCD). µ-RS spectra are analyzed using Labspec 5.0 software.

3. Results and Discussion

Prior to inducing the oxidation of the metallic wires, characterization of the electrical resistivity has been performed. The variation of the resistance (R) with length (L) of the wire is determined using a 4-point probe configuration, and the data are plotted in Figure 2a.
Then, a linear fit of the data is applied to calculate the resistivity ( ρ ) of the Nb metal wire by using Ohm’s law:
I = V R
R = ρ L S    
where S is the section of the wire. The obtained resistivity value is ρ = 1.54 ± 0.31 × 10 7 Ω · m , which matches the expected value for the resistivity of pure niobium at room temperature [26].
Once the wire is mounted on the growing setup (Figure 1a) and a high-density current is made to go through it, this value of resistivity is increased. This is related to several factors: temperature increase due to Joule heating, linear expansion of the material due to temperature, and section reduction due to oxide formation on the surface. So, the current source needs to increase the voltage in order to maintain the fixed current, as observed in the measurements of Table 1. As the section of the metallic wire decreases, higher probability of failure and breaking of the wire is expected, which affects how long the treatment can last. This explains why the time can be expanded for 60 s and more for the lower values of current in Table 1, whereas times longer than 30 s cannot be maintained for the highest current (5.5 A).
The selected growing parameters allow us to study the evolution of the obtained oxide with current value and time. We observe the formation of niobium oxide in two different scales: nanowires on the surface and the micrometric oxide layer covering the metallic wire (Figure 2b). We start with the description of the nanowires.
The evolution of the nanowires with current value, keeping a fixed growing time of 60 s, is shown in Figure 3. For 3.5 A, there is no formation of any nanostructure on the Nb metal wire surface. The formation of nanowires is observed for currents above 4.5 A, whereas for current values between 4.1 and 4.5 A, nucleation points can be identified (Figure 3a), as well as some isolated nanowires evenly formed, but with low reproducibility of the final growth. As the current increases, the density, length, and diameter of the nanowires increase (Figure 3b–d). Nanowires are thicker at the base (hundreds of nm) than at the tip (below 100 nm), and they have lengths of a few microns. The best current condition for obtaining a high density of nanowires with high aspect ratio (diameter vs. length) is 4.8 A. At higher currents, nanowires start to evolve to microrods (Figure 3d). The temperatures reached by the Nb metal wire are comparable to those reported for the growth of niobium oxide nanowires on metal foils by thermal treatment [11,12,13], but the times are clearly shorter. Thus, the rapid growth of the nanowires could be related to an increase in the diffusion rate of oxygen and niobium mobility due to electromigration [27].
Then, we study the evolution of the nanowires with time for a fixed current value of 4.8 A (Figure 4). The features of the evolution are similar to those observed for the evolution with current. For a growing time of 5 s (Figure 4a), nucleation points and tiny nanowires start to appear, but evenly distributed. A high density of nanowires with good aspect ratio is obtained for times between 15 s and 60 s (Figure 4b–d). Above 60 s (Figure 4e), the behavior is comparable with the case of 5.0 A in Figure 3d, i.e., nanowires evolve into microrods. It is also interesting to note that the length of the nanowires or rods does not exceed 5 microns, and no appreciable change is observed when increasing from 60 s to 120 s, as in Figure 4, or from 4.8 to 5.0 A, as in Figure 3. This may be an indication of the steps of growth: first nanowires are formed, and their growth is then slowed down due to the formation of the micrometric oxide layer.
The formation of microrods is clearly achieved for current values of 5.5 A (Figure 5a). These microrods have diameters and lengths of a few microns. On the other hand, for this level of current it is possible to visualize the formation of a micrometric oxide layer by studying the cross-section of the wire (Figure 5b). In Figure 5b, the measured oxide layer thickness is around 60 μm, whereas the metallic core diameter has been reduced to 220 μm. It is expected that the thickness of these layers varies with current and time, as observed for the nanowires. We present the results of these experiments in Figure 6 (current evolution) and Figure 7 (time evolution).
SEM images in Figure 6 and Figure 7 are presented along with the EDX maps of oxygen (cyan) and niobium (red). In both figures, two regions in the Nb wire can be identified, in agreement with the sketch in Figure 3: a metallic core, where only a niobium signal is detected, and an oxide layer, where both an oxygen and niobium signal are observed. For both current and time evolutions, an increase in the thickness of the oxide layer is clear, associated with a decrease in the diameter of the metallic core. This behavior results from a diffusion phenomenon of oxygen towards the metallic core. It is well known that diffusion rate increases with temperature (higher current means higher temperature) and with time, as derived from Fick’s laws and the diffusion coefficient with temperature.
The formation of the oxide layer is almost symmetric around the metallic core, as seen in Figure 6 and Figure 7. To measure the value of the size of the core and the layer, we have measured the height and width, considering the elliptical shape, and the mean values of both measurements are presented in Figure 8. An increase in time of treatment produces an increase in the thickness of the oxide layer (Figure 8a). This effect is also observed for an increase in current (Figure 8b). On the other hand, the formation of the oxide produces a reduction of the metallic core (Figure 8c–d). The oxidation of the metal produces an increase in the total volume of material [28], as Nb2O5 has close to half the density (4.6 g/cm3) of Nb metal (8.6 g/cm3). This ratio agrees with the measured values shown in Figure 8, mainly for the largest oxide layers. For example, for the fixed current of 4.8 A, the metallic core diameter is reduced from 250 μm to 217 μm (i.e., a reduction of 33 μm) and the oxide layer has a thickness of around 62 μm. The evolution observed with current (which is directly related to the temperature reached) and time is reasonable considering that the growth process is driven by oxygen diffusion from the atmosphere through the oxide layer into the Nb metal [29].
The diffusion coefficients D for oxygen in Nb metal and in Nb2O5 vary with temperature, following the equations [30,31]:
O x y g e n   i n   N b :                   D = 5.3 × 10 7 e x p 1.095 × 10 5 R T  
O x y g e n   i n   N b 2 O 5 :             D = 1.72 × 10 6 e x p 2.07 × 10 6 R T
where the pre-exponential coefficient is expressed in m2/s and the activation energy in J/mol. From these equations, it is clear that the diffusion rate of oxygen is higher in Nb metal than in the oxide. If we calculate the penetration depth ( L p = D t ) of oxygen for different temperature, we can estimate the depth to which diffusion is significant. For the case of oxygen in Nb, the penetration depths are calculated in Table 2 for different times and temperatures. If we compare these values with the values of reduction of the metallic core, we can see that, if only oxygen diffusion in Nb metal is taken into account, the amount of Nb converted into oxide should be higher. We propose that, in a first stage, an oxide layer is produced through oxygen diffusion from air towards the metallic material. Once this oxide layer is formed, the growth rate would be restricted by the oxygen transference through the oxide, which is much slower. This could explain the almost linear behavior observed for the oxide thickness with time and current (i.e., temperature). Similar behavior was observed in previous studies on the oxidation of niobium by heat treatments [29,32,33]. For example, Kofstad and Kjollesdal [32] associated the linear kinetics with a rate-determining transport of oxygen ions through an oxide barrier next to the metal. In general, a complex evolution of the oxidation of Nb is observed depending on temperature or oxygen partial pressure, as many variables are involved, e.g., the competition of oxygen diffusion though different Nb2O5 polymorphism or the appearance of short-circuit paths for diffusion through the oxide layer [29].
Once the growth behavior is determined, we perform XRD and µ-RS measurements in order to assess the type of oxide that is formed. The typical XRD pattern recorded is shown in Figure 9. XRD measurements are performed on the material forming the oxide layer by separating this oxide from the metallic core, giving us information about the main phase of the oxide formed. For all the selected growth conditions where oxide is formed, the diffraction maxima can be associated with the H-Nb2O5 monoclinic phase (ICDD card no. 00-037-1468). This observation is coherent with the measured temperatures during the growth (Table 1). Oxide layer and nanowires appear for currents above 4.1 A, i.e., for temperatures well above 900 °C, which is the condition for forming the H-Nb2O5 phase [5].
To obtain more information about the formed oxide at a micrometric level, µ-RS measurements are carried out on the surface as well as on the cross-section of the Nb metal wires. The spectra measured on the surface where nanowires are formed for different current values are presented in Figure 9b. All of them correlated well with the expected results for H-Nb2O5 phase due to the growing temperature [14,34,35]. Three frequency regions can be identified. First, below 200 cm−1, modes are related to external lattice vibrations (for which the octahedron is considered as a rigid unit) [36]. Between 200 cm−1 and 500 cm−1, modes related to bending of the Nb-O bodings in the [NbO6] octahedra are found [34,37,38]. Between 500 and 800 cm−1, the bands are associated with stretching vibrations in the [NbO6] octahedra [34]. In general, several modes are detected as the octahedra in the Nb2O5 structure are slightly distorted. Finally, the band located at 992 cm−1 is generally ascribed to the symmetric stretching modes of the terminal bonds of Nb=O in octahedra with a high degree of distortion [34,37], which are related to the existence of shear planes (edge-shared octahedra) in H-Nb2O5 [38,39]. The main difference observed with the current variation is an increase in the definition of some of the Raman bands, mainly in the low- and medium-frequency region. This phenomenon is observed for an increased crystal quality or a reduction of oxygen deficiency [40], as well as for an increase in the crystalline size [35], which is in agreement with our SEM observations of the samples. Separated nanowires show similar Raman spectra associated with the H-Nb2O5 phase (Figure 10a).
For the wires oxidized with the higher values of current (i.e., 5.0 A and 5.5 A), a variation of the RS signal is observed along the length of the wire (Figure 10). Considering that the temperature reached at the nanowire has a profile that decreases towards the electrodes (see Figure 1b), we record the spectra at the center of the wire (2.5 cm from the electrode, ‘high’ temperature in Figure 10b,c); at 1.25 cm from the electrode (‘medium’ temperature); and at 0.7 cm from the electrode (‘low’ temperature). In the Raman spectra, we observe less defined bands as we move away from the center of the Nb metallic wire. This is in agreement with a reduction in the crystal quality or the increase of structures in the nanometric scale. An inspection of the structures obtained along the metallic wire in the selected positions indicate that, as the temperature profile reduces, the structures evolve towards nanowires, in an evolution similar to the one observed for the current variation (Figure 4 and Figure 9b).
Finally, we study the Raman signal recorded on the cross-section of a Nb wire, to check if there is any modification along the thickness of the oxide layer. The optical section of the metallic wire (Figure 11a) allows us to identify the oxide layer (white in the optical micrograph) and the metallic core (dark blue in the micrograph). The line profile of the evolution of the Raman spectra is shown in Figure 11b. In the graph, the position at which the spectrum is recorded (Y-axis) is presented in terms of Raman shift (X-axis) and intensity of the Raman signal (Z-axis). Similar RS bands are recorded along the thickness of the layer, confirming that the oxide layer is uniform in crystal structure. No signal related to sub-oxides (NbO, NbO2) is detected. Spectra recorded at selected points are presented in Figure 11c. At the center of the metallic core, no RS signal is obtained, as it is a metal without oxidation. On the other hand, the RS signal recorded along the oxide layer shows the same features as on the surface (see Figure 9b). It is at the boundary between the oxide and the metallic core that some changes in the spectra are seen, mainly on the spectrum recorded at the boundary on the side of the metal (‘boundary in’). Even on a region that appears metallic in the optical micrograph, an oxide signal is still detectable, confirming that oxygen is diffusing inside the metal to form new oxide layers.

4. Conclusions

In this work, we have described the formation of Nb2O5 nanowires and micrometric oxide layers on Nb metal wires. The synthesis method is based on conducting a high electrical current density through the Nb wire, increasing the temperature of the material by Joule heating. Growth can be produced in times shorter than 1 min by controlling the current density. The formation of Nb2O5 nanowires on the Nb wire metal is produced by the diffusion of atmospheric oxygen inside the metal, assisted by electromigration. On the other hand, the formation of the micrometric oxide layer seems to be initially controlled by the diffusion of oxygen atoms in Nb, and after the first oxide is formed, by the diffusion of oxygen through the oxide layer into the metal. The XRD and RS characterizations confirm the formation of H-Nb2O5 phase, in agreement with the temperature reached in the metal when the current is flowing.

Author Contributions

Conceptualization, B.S. and P.F.; methodology, A.C.-V. and B.S.; software, A.C.-V. and B.S.; validation, A.C.-V., B.S. and P.F.; formal analysis, B.S. and A.C.-V.; investigation, A.C.-V. and B.S.; resources, P.F.; data curation, B.S.; writing—original draft preparation, B.S.; writing—review and editing, A.C.-V., P.F. and B.S.; visualization, A.C.-V., P.F. and B.S.; supervision, B.S. and P.F.; project administration, P.F. and B.S.; funding acquisition, P.F. and B.S. All authors have read and agreed to the published version of the manuscript.

Funding

The authors are grateful to the Comunidad de Madrid for support via the Project PR65/19-22464 (Proyectos de I+D para jóvenes doctores) and to Complutense University of Madrid for support via the Project PR3/23-30813.

Data Availability Statement

Data are contained within the article. The raw data supporting the conclusions of this article will be made available by the authors on request.

Conflicts of Interest

The authors declare no conflicts of interest.

References

  1. Yuan, S.; Duan, X.; Liu, J.; Ye, Y.; Lv, F.; Liu, T.; Wang, Q.; Zhang, X. Recent Progress on Transition Metal Oxides as Advanced Materials for Energy Conversion and Storage. Energy Storage Mater. 2021, 42, 317–369. [Google Scholar] [CrossRef]
  2. Danish, M.S.S.; Estrella, L.L.; Alemaida, I.M.A.; Lisin, A.; Moiseev, N.; Ahmadi, M.; Nazari, M.; Wali, M.; Zaheb, H.; Senjyu, T. Photocatalytic Applications of Metal Oxides for Sustainable Environmental Remediation. Metals 2021, 11, 80. [Google Scholar] [CrossRef]
  3. Sawa, A. Resistive Switching in Transition Metal Oxides. Mater. Today 2008, 11, 28–36. [Google Scholar] [CrossRef]
  4. Dey, A. Semiconductor Metal Oxide Gas Sensors: A Review. Mater. Sci. Eng. B Solid. State Mater. Adv. Technol. 2018, 229, 206–217. [Google Scholar] [CrossRef]
  5. Nico, C.; Monteiro, T.; Graça, M.P.F. Niobium Oxides and Niobates Physical Properties: Review and Prospects. Prog. Mater. Sci. 2016, 80, 1–37. [Google Scholar] [CrossRef]
  6. Su, K.; Liu, H.; Gao, Z.; Fornasiero, P.; Wang, F. Nb2O5-Based Photocatalysts. Adv. Sci. 2021, 8, 2003156. [Google Scholar] [CrossRef]
  7. He, J.; Hu, Y.; Wang, Z.; Lu, W.; Yang, S.; Wu, G.; Wang, Y.; Wang, S.; Gu, H.; Wang, J. Hydrothermal Growth and Optical Properties of Nb2O5 Nanorod Arrays. J. Mater. Chem. C Mater. 2014, 2, 8185–8190. [Google Scholar] [CrossRef]
  8. Liu, M.; Yan, C.; Zhang, Y. Fabrication of Nb2O5 Nanosheets for High-Rate Lithium Ion Storage Applications. Sci. Rep. 2015, 5, 8326. [Google Scholar] [CrossRef]
  9. Qi, S.; Zuo, R.; Liu, Y.; Wang, Y. Synthesis and Photocatalytic Activity of Electrospun Niobium Oxide Nanofibers. Mater. Res. Bull. 2013, 48, 1213–1217. [Google Scholar] [CrossRef]
  10. Graça, M.P.F.; Meireles, A.; Nico, C.; Valente, M.A. Nb2O5 Nanosize Powders Prepared by Sol–Gel—Structure, Morphology and Dielectric Properties. J. Alloys Compd. 2013, 553, 177–182. [Google Scholar] [CrossRef]
  11. Varghese, B.; Haur, S.C.; Lim, C.T. Nb2O5 Nanowires as Efficient Electron Field Emitters. J. Phys. Chem. C 2008, 112, 10008–10012. [Google Scholar] [CrossRef]
  12. Wang, Z.; Hu, Y.; Wang, W.; Zhang, X.; Wang, B.; Tian, H.; Wang, Y.; Guan, J.; Gu, H. Fast and Highly-Sensitive Hydrogen Sensing of Nb2O5 Nanowires at Room Temperature. Int. J. Hydrogen Energy 2012, 37, 4526–4532. [Google Scholar] [CrossRef]
  13. Lim, J.H.; Choi, J. Formation of Niobium Oxide Nanowires by Thermal Oxidation. J. Ind. Eng. Chem. 2009, 15, 860–864. [Google Scholar] [CrossRef]
  14. Sotillo, B.; López, F.A.; Alcaraz, L.; Fernández, P. Characterization of Nb22O54 Microrods Grown from Niobium Oxide Powders Recovered from Mine Tailings. Ceram. Int. 2021, 47, 13859–13864. [Google Scholar] [CrossRef]
  15. Mozetič, M.; Cvelbar, U.; Sunkara, M.K.; Vaddiraju, S. A Method for the Rapid Synthesis of Large Quantities of Metal Oxide Nanowires at Low Temperatures. Adv. Mater. 2005, 17, 2138–2142. [Google Scholar] [CrossRef]
  16. Urbieta, A.; Sánchez, V.; Fernández, P.; Piqueras, J. Fast Growth of Undoped and Sn- and Tb-Doped ZnO Nanowires by Joule Heating of Zn. CrystEngComm 2018, 20, 4449–4454. [Google Scholar] [CrossRef]
  17. Rackauskas, S.; Nasibulin, A.G.; Jiang, H.; Tian, Y.; Kleshch, V.I.; Sainio, J.; Obraztsova, E.D.; Bokova, S.N.; Obraztsov, A.N.; Kauppinen, E.I. A Novel Method for Metal Oxide Nanowire Synthesis. Nanotechnology 2009, 20, 165603. [Google Scholar] [CrossRef]
  18. Criado, D.; Zúñiga, A. Influence of an Electric Current on the Growth Kinetics of CuO Nanowires Produced by Oxidation. Mater. Today Commun. 2019, 19, 18–22. [Google Scholar] [CrossRef]
  19. Rodríguez, B.; Hidalgo, P.; Piqueras, J.; Méndez, B. Influence of an External Electric Field on the Rapid Synthesis of MoO3 Micro- and Nanostructures by Joule Heating of Mo Wires. RSC Adv. 2020, 10, 11892–11897. [Google Scholar] [CrossRef]
  20. Rodríguez, B.; Dolado, J.; López-Sánchez, J.; Hidalgo, P.; Méndez, B. Room Temperature Polymorphism in WO3 Produced by Resistive Heating of W Wires. Nanomaterials 2023, 13, 884. [Google Scholar] [CrossRef]
  21. Ramos-Justicia, J.F.; Urbieta, A.; Fernández, P. Rapid Growth of Metal–Metal Oxide Core–Shell Structures through Joule Resistive Heating: Morphological, Structural, and Luminescence Characterization. Materials 2024, 17, 208. [Google Scholar] [CrossRef]
  22. Ramos-Justicia, J.F.; Ballester-Andújar, J.L.; Urbieta, A.; Fernández, P. Growth of Zr/ZrO2 Core–Shell Structures by Fast Thermal Oxidation. Appl. Sci. 2023, 13, 3714. [Google Scholar] [CrossRef]
  23. Piqueras, J.; Hidalgo, P. Growth of Metal Oxide Nanostructures by Thermal Oxidation of Metals Under Influence of External Electric Fields and Electric Current Flow. Phys. Status Solidi 2021, 218, 2100323. [Google Scholar] [CrossRef]
  24. Fang, W.; Zhang, Y.; Kang, C.; Meng, Q.; Shi, A.; Lou, S.; Cheng, X.; Yin, G.; Zhang, L. Oxygen Vacancies Nb2O5-x: Ultrastable Lithium Storage Anode Materials for Advanced Rechargeable Batteries. Appl. Surf. Sci. 2022, 600, 154068. [Google Scholar] [CrossRef]
  25. Sheng, Y.; Wang, Y.; Yin, S.; Zhao, L.; Zhang, X.; Liu, D.; Wen, G. Niobium-Based Oxide for Anode Materials for Lithium-Ion Batteries. Chem. A Eur. J. 2023, e202302865. [Google Scholar] [CrossRef]
  26. Satya Prasad, V.V.; Baligidad, R.G.; Gokhale, A.A. Niobium and Other High Temperature Refractory Metals for Aerospace Applications. In Aerospace Materials and Material Technologies: Volume 1: Aerospace Materials; Springer: Berlin/Heidelberg, Germany, 2017; pp. 267–288. [Google Scholar]
  27. Zhang, L.; Li, J.; Xiong, D.; Xu, M.; Yin, L.; Zhang, H.; Yao, Z. Dynamic Growth Mechanism of Tin Whisker Driven by Compressive Stress under Thermal-Mechanic-Electric-Diffusion Coupling. Vacuum 2023, 215, 112299. [Google Scholar] [CrossRef]
  28. Douglass, D.L. The Thermal Expansion of Niobium Pentoxide and Its Effect on the Spalling of Niobium Oxidation Films. J. Less Common. Met. 1963, 5, 151–157. [Google Scholar] [CrossRef]
  29. Seybolt, A.U. Oxidation of Metals. Adv. Phys. 1963, 12, 1–43. [Google Scholar] [CrossRef]
  30. Chen, W.K.; Jackson, R.A. Diffusion of Oxygen in Near-Stoichiometric A-Nb2O5. J. Chem. Phys. 1967, 47, 1144–1148. [Google Scholar] [CrossRef]
  31. Boratto, F.J.M.; Reed-Hill, R.E. On the Calculations of the Diffusion Coefficients of Oxygen and Nitrogen in Niobium. Metall. Trans. A 1977, 8, 1233–1238. [Google Scholar] [CrossRef]
  32. Kofstad, P.; Kjollesdal, H. Oxidation of Niobium (Columbium) in the Temperature Range 500 to 1200 C. Trans. Met. Soc. AIME 1961, 221, 285. [Google Scholar]
  33. Sheasby, J.S. The Oxidation of Niobium in the Temperature Range 450–720 °C. J. Electrochem. Soc. 1968, 115, 695. [Google Scholar] [CrossRef]
  34. Jehng, J.M.; Wachs, I.E. Structural Chemistry and Raman Spectra of Niobium Oxides. Chem. Mater. 1991, 3, 100–107. [Google Scholar] [CrossRef]
  35. Soares, M.R.N.; Leite, S.; Nico, C.; Peres, M.; Fernandes, A.J.S.; Graça, M.P.F.; Matos, M.; Monteiro, R.; Monteiro, T.; Costa, F.M. Effect of Processing Method on Physical Properties of Nb2O5. J. Eur. Ceram. Soc. 2011, 31, 501–506. [Google Scholar] [CrossRef]
  36. McConnell, A.A.; Aderson, J.S.; Rao, C.N.R. Raman Spectra of Niobium Oxides. Spectrochim. Acta A 1976, 32, 1067–1076. [Google Scholar] [CrossRef]
  37. Ikeya, T.; Senna, M. Change in the Structure of Niobium Pentoxide Due to Mechanical and Thermal Treatments. J. Non Cryst. Solids 1988, 105, 243–250. [Google Scholar] [CrossRef]
  38. Andersson, S.; Galy, J. Wadsley Defects and Crystallographic Shear in Hexagonally Close-Packed Structures. J. Solid. State Chem. 1970, 1, 576–582. [Google Scholar] [CrossRef]
  39. Cava, R.J.; Batlogg, B.; Krajewski, J.J.; Poulsen, H.F.; Gammel, P.; Peck, W.F.; Rupp, L.W. Electrical and Magnetic Properties of Nb2O5-δ Crystallographic Shear Structures. Phys. Rev. B 1991, 44, 6973–6981. [Google Scholar] [CrossRef]
  40. Sotillo, B.; Ariza, R.; Fernández, P.; Solis, J. Ultrafast-Laser Powder Bed Fusion of Oxygen-Deficient Nb2O5 Ceramics with Highly Improved Electrical Properties. Mater. Des. 2022, 224, 111346. [Google Scholar] [CrossRef]
Figure 1. (a) Sketch of the setup used to grow the Nb2O5 samples. (b) Photograph of the wire while current is flowing.
Figure 1. (a) Sketch of the setup used to grow the Nb2O5 samples. (b) Photograph of the wire while current is flowing.
Crystals 14 00245 g001
Figure 2. (a) Electrical characterization of pristine Nb metal wires. (b) Sketch of the cross-section of a Nb wire after the growth process.
Figure 2. (a) Electrical characterization of pristine Nb metal wires. (b) Sketch of the cross-section of a Nb wire after the growth process.
Crystals 14 00245 g002
Figure 3. SEM images showing the evolution of Nb2O5 structures with current value of (a) 4.1 A; (b) 4.5 A; (c) 4.8 A; and (d) 5.0 A (t = 60 s).
Figure 3. SEM images showing the evolution of Nb2O5 structures with current value of (a) 4.1 A; (b) 4.5 A; (c) 4.8 A; and (d) 5.0 A (t = 60 s).
Crystals 14 00245 g003
Figure 4. SEM images showing the evolution of Nb2O5 structures with time (a) 5 s; (b) 15 s; (c) 30 s; (d) 60 s; and (e) 120 s (I = 4.8 A).
Figure 4. SEM images showing the evolution of Nb2O5 structures with time (a) 5 s; (b) 15 s; (c) 30 s; (d) 60 s; and (e) 120 s (I = 4.8 A).
Crystals 14 00245 g004
Figure 5. (a) SEM image of microrods obtained with a current value of 5.5 A. (b) SEM image of the cross-section of a Nb wire after the oxidation process at 5.5 A, showing the oxide layer that has been produced on the metallic core.
Figure 5. (a) SEM image of microrods obtained with a current value of 5.5 A. (b) SEM image of the cross-section of a Nb wire after the oxidation process at 5.5 A, showing the oxide layer that has been produced on the metallic core.
Crystals 14 00245 g005
Figure 6. Evolution of Nb2O5 oxide layer with current value of (a) 3.5 A; (b) 4.1 A; (c) 4.5 A; and (d) 5.0 A (t = 60 s). EDX maps show the distribution of Niobium (red) and Oxygen (cyan).
Figure 6. Evolution of Nb2O5 oxide layer with current value of (a) 3.5 A; (b) 4.1 A; (c) 4.5 A; and (d) 5.0 A (t = 60 s). EDX maps show the distribution of Niobium (red) and Oxygen (cyan).
Crystals 14 00245 g006
Figure 7. Evolution of Nb2O5 oxide layer with time (a) 5 s; (b) 15 s; (c) 60 s; and (d) 120 s (I = 4.8 A). EDX maps show the distribution of Niobium (red) and Oxygen (cyan).
Figure 7. Evolution of Nb2O5 oxide layer with time (a) 5 s; (b) 15 s; (c) 60 s; and (d) 120 s (I = 4.8 A). EDX maps show the distribution of Niobium (red) and Oxygen (cyan).
Crystals 14 00245 g007
Figure 8. Plot of the evolution of the mean value of the oxide layer thickness (a) and the metallic core diameter (c) with time, for a fixed current of 4.8 A. In (b,d), the evolution is shown in terms of current for a fixed time value of 60 s.
Figure 8. Plot of the evolution of the mean value of the oxide layer thickness (a) and the metallic core diameter (c) with time, for a fixed current of 4.8 A. In (b,d), the evolution is shown in terms of current for a fixed time value of 60 s.
Crystals 14 00245 g008
Figure 9. (a) Diffractogram of the oxide obtained on the Nb metal wires by Joule resistive heating. (b) µ-RS measurements performed at the surface with nanowires for different current values.
Figure 9. (a) Diffractogram of the oxide obtained on the Nb metal wires by Joule resistive heating. (b) µ-RS measurements performed at the surface with nanowires for different current values.
Crystals 14 00245 g009
Figure 10. (a) Raman spectrum of individual nanowires protruding from the oxide layer. The peak at 520 cm−1 is related to the silicon substrate. (b) µ-RS variation along the Nb metal wire for 5.5 A and 30 s. (c) Morphology evolution of the nanowires.
Figure 10. (a) Raman spectrum of individual nanowires protruding from the oxide layer. The peak at 520 cm−1 is related to the silicon substrate. (b) µ-RS variation along the Nb metal wire for 5.5 A and 30 s. (c) Morphology evolution of the nanowires.
Crystals 14 00245 g010
Figure 11. (a) Optical micrograph of the cross-section of a Nb wire oxidized with a current of 5.0 A. (b) Intensity profile of Raman spectra recorded along a line on points towards the oxide layer cross-section. (c) Selected Raman spectra measured on the cross-section of a Nb metal wire.
Figure 11. (a) Optical micrograph of the cross-section of a Nb wire oxidized with a current of 5.0 A. (b) Intensity profile of Raman spectra recorded along a line on points towards the oxide layer cross-section. (c) Selected Raman spectra measured on the cross-section of a Nb metal wire.
Crystals 14 00245 g011
Table 1. Conditions used for growing the samples.
Table 1. Conditions used for growing the samples.
SampleCurrent (A)Time (s)Voltage Interval (V)Max. Temperature (°C)
1a3.5601.9–2.0680
2a4.1302.6–2.71000
2b 602.6–2.9
3a4.5302.8–3.01100
3b 603.0–3.5
4a4.853.51150
4b 153.3–3.5
4c 303.4–3.8
4d 603.3–4.3
5a5.053.71200
5b 153.6–4.0
5c 303.5–4.1
5d 603.4–4.7
6a5.5154.3–5.11360
7b 304.2–6.4
Table 2. Penetration depths ( L p = D t ) for oxygen in Nb calculated for different temperatures and times, using diffusion coefficient of Equation (3).
Table 2. Penetration depths ( L p = D t ) for oxygen in Nb calculated for different temperatures and times, using diffusion coefficient of Equation (3).
T (°C)t = 5 st = 15 st = 30 s t = 60 s
6501.3 μm2.2 μm3.2 μm4.5 μm
9005.9 μm 10.3 μm14.5 μm20.6 μm
10009.2 μm16.0 μm22.6 μm32.0 μm
110013.4 μm23.3 μm32.9 μm46.6 μm
120018.6 μm32.3 μm45.6 μm64.5 μm
130024.7 μm42.9 μm69.6 μm85.7 μm
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content.

Share and Cite

MDPI and ACS Style

Calvo-Villoslada, A.; Fernández, P.; Sotillo, B. Rapid Growth of Niobium Oxide Nanowires by Joule Resistive Heating. Crystals 2024, 14, 245. https://doi.org/10.3390/cryst14030245

AMA Style

Calvo-Villoslada A, Fernández P, Sotillo B. Rapid Growth of Niobium Oxide Nanowires by Joule Resistive Heating. Crystals. 2024; 14(3):245. https://doi.org/10.3390/cryst14030245

Chicago/Turabian Style

Calvo-Villoslada, Aarón, Paloma Fernández, and Belén Sotillo. 2024. "Rapid Growth of Niobium Oxide Nanowires by Joule Resistive Heating" Crystals 14, no. 3: 245. https://doi.org/10.3390/cryst14030245

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.

Article Metrics

Back to TopTop