Article

Characterization of Residual Stress in SOI Wafers by Using MEMS Cantilever Beams

1
School of Mechano-Electronic Engineering, Xidian University, Xi’an 710071, China
2
City U-Xidian Joint Laboratory of Micro/Nano-Manufacturing, Shenzhen 518057, China
3
Xi’an Chuanglian Electronic Component (Group) Co., Ltd., Xi’an 710065, China
4
School of Mechanical Engineering, University of Birmingham, Birmingham B15 2TT, UK
*
Author to whom correspondence should be addressed.
These authors contributed equally to this work.
Micromachines 2023, 14(8), 1510; https://doi.org/10.3390/mi14081510
Submission received: 30 June 2023 / Revised: 22 July 2023 / Accepted: 23 July 2023 / Published: 27 July 2023
(This article belongs to the Section A:Physics)

Abstract

:
Silicon-on-insulator (SOI) wafers are crucial raw materials in the manufacturing process of microelectromechanical systems (MEMS). Residual stresses generated inside the wafers during the fabrication process can seriously affect the performance, reliability, and yield of MEMS devices. In this paper, a low-cost method based on mechanical modeling is proposed to characterize the residual stresses in SOI wafers in order to calculate the residual stress values based on the deformation of the beams. Based on this method, the residual strain of the MEMS beam, and thus the residual stress in the SOI wafer, were experimentally determined. The results were also compared with the residual stress results calculated from the deflection of the rotating beam to demonstrate the validity of the results obtained by this method. This method provides valuable theoretical reference and data support for the design and optimization of devices based on SOI-MEMS technology. It provides a lower-cost solution for the residual stress measurement technique, making it available for a wide range of applications.

1. Introduction

The residual stress in silicon-on-insulator (SOI) wafers has been a significant concern impacting the reliability of microsystem devices and the performance of MEMS devices, potentially leading to device failure [1]. Therefore, it is essential to study the residual stress in MEMS devices. For devices based on SOI-MEMS technology, the residual stress primarily arises from two sources: residual stress in the SOI wafer and residual stress formed during the processing of MEMS devices. While previous research has focused on residual stress in thin layers [2,3,4,5], or residual stress generated during processing [6,7,8,9], there is limited research on the residual stress in SOI chips themselves.
Residual stress testing methods can be broadly categorized as either destructive or non-destructive. Destructive methods release stress by mechanically separating or splitting the components on the surface. Recently, optical techniques [10,11,12,13], digital image processing [14,15,16], and incremental hole-drilling methods [17] have been extended to characterize residual stresses with high accuracy. However, these techniques are not suitable for measuring residual stresses in micro and nano devices or SOI-MEMS devices due to their destructive nature, which can cause material damage and yielding.
Non-destructive measurement methods for residual stress have made significant progress in recent years. These include radiation methods [18,19], nanoindentation strain methods [20], and residual strain measurement methods [21,22], among others. For example, E. Dobročka et al. [18] developed a method to measure residual stress in strongly woven ZnO layers using X-ray diffraction stress analysis, achieving high accuracy. However, radiation methods suffer from shallow measurement depth and high costs. On the other hand, nanoindentation is a popular technique due to its low damage and ease of measurement. However, different theoretical calculation models used in nanoindentation yield different results in mechanical energy properties such as contact area, material hardness, and stress. Commonly used nanoindentation theory calculation models include the Suresh theory model [23], Lee model [24], Swadener theory model [25], and Xu model [26].
To overcome these challenges, this study introduces a non-contact method to characterize the residual stress in SOI-MEMS devices. The residual strain measurement method calculates the residual stress value by measuring the residual strain and applying theoretical calculations based on mechanical equations. As a non-destructive measurement method, it has received much attention in recent years due to its scalability. The proposed method in this paper utilizes theoretical calculations and bending moment measurements to accurately assess the residual stress. By examining the underlying mechanisms of residual stress generation in SOI wafers, mechanical deflection models for MEMS cantilever beams and fixed beams are developed. Experimental testing is conducted to validate the effectiveness and feasibility of this method for characterizing residual stress in SOI wafers.

2. Mechanism Analysis of Residual Stress in SOI Wafer

Silicon direct bonding (SDB) technology is widely used in the preparation of SOI wafers. The process involved in creating bonded SOI wafers is illustrated in Figure 1 [27,28]. It typically begins with a wet chemical and ultrasonic cleaning of the silicon wafers, which include the device wafer and the handle wafer. Following this, the device layer undergoes thermal oxidation to create a surface oxide layer, which ultimately becomes the buried oxide in the SOI structure. The two wafers are then pre-bonded in an ultra-clean environment. The next step involves annealing the bonded wafer pairs at temperatures in the range of 1100–1200 °C. This process promotes the formation of strong Si-O-Si or Si-Si bonds, ensuring a permanent bond between the wafers. Finally, the device layer is polished to achieve the desired thickness.
The SDB technology offers several advantages in the preparation of SOI wafers. It allows for the creation of a thin and defect-free buried oxide layer, which is crucial for the performance of SOI devices. The bonding process enables the integration of different materials and the formation of high-quality interfaces. Additionally, the ability to control the thickness of the device layer through polishing allows for customization according to specific device requirements.
The process of thermal oxidation, which involves growing a SiO2 layer on the surface of a polished silicon wafer, induces the generation of residual stresses within the layer. These residual stresses can be categorized into thermal stress and intrinsic stress [22,23]. Thermal stress, also known as thermal mismatch stress, arises due to the disparity in the thermal expansion coefficients between the layer and the substrate material. On the other hand, intrinsic stress is more complex in nature, primarily attributed to the mismatch in lattice structures between the layer and the substrate material [4], as depicted in Figure 2 [29]. The lattice mismatch leads to the formation of edge dislocations, and these dislocations create an associated elastic stress field around them.
During the thermal growth of the SiO2 layer on the polished silicon wafer surface, a significant amount of oxygen atoms is introduced into the silicon surface, leading to volume expansion. However, since the grown SiO2 layer is bonded to the substrate, its perimeter cannot freely expand. Considering that the thickness of the substrate is much larger than that of the SiO2 layer, it can be assumed that the radial expansion of the SiO2 layer is nearly zero. As a result, the SiO2 layer can only expand in the direction perpendicular to the substrate surface, resulting in the presence of intrinsic compressive stress distributed in a gradient along the thickness direction of the SiO2 layer.
During the subsequent cooling process, the SiO2 layer experiences a uniformly distributed thermal mismatch stress. This is because the thermal expansion coefficient of SiO2 is lower than that of silicon. After the growth of the SiO2 layer, the residual stress within the layer is a combination of the thermal mismatch stress and the intrinsic stress. At this point, the SiO2 layer and the silicon substrate reach equilibrium, and tensile stress is present in the substrate. The distribution of residual stress in the layer and substrate is illustrated in Figure 3.
In the prepared SOI wafer, the distribution of residual stress within the wafer is depicted in Figure 4. The SiO2 layer experiences compressive stress from the underlying silicon and the device layer, while the underlying silicon and the device layer undergo tensile stress from the SiO2 layer. The residual stress in the SiO2 layer and the device layer exhibits a gradient along the thickness direction. On the other hand, since the thickness of the underlying silicon is considerably larger than the thickness of the other two layers, the residual stress in the underlying silicon can be approximated as uniformly distributed.

3. Mechanical Theoretical Modeling

In the processing of MEMS devices using the SOI wafer structure, the gradual release of the underlying silicon and SiO2 layers disrupts the original stress balance mechanism within the SOI structure, leading to the development of residual stress. This residual stress induces bending deformation in the MEMS devices, subsequently impacting their performance and reliability. When processing a cantilever beam using the SOI wafer, initially, before the release of the substrate layer and the SiO2 layer in the three-layer SOI structure, the cantilever beam is in an ideal state of stress balance due to the mutual constraint exerted by the layers of the SOI wafer, as depicted in Figure 5a. Since the residual stress σ in the cantilever beam exhibits a stress gradient along the thickness direction, this stress gradient can be approximated as the superposition of stress σ0 and σ1, as illustrated in Figure 5b.
Prior to the release of the substrate, a shear stress F1 exists within the SiO2 layer to counterbalance the residual stress of the substrate, as depicted in Figure 6a. Since the shear force F1 is an eccentric force, it generates a stress gradient within the SiO2 layer while laterally restraining the layer from stretching. Consequently, after the substrate is released, the influence of the shear force F1 on the SiO2 layer is also eliminated, and the lateral constraint on the cantilever beam at the lower end of the SiO2 layer disappears. This results in lateral elongation   Δ l S i O 2 of the SiO2 layer and, concurrently, because of the stress gradient, a moment is generated, leading to deformation y1 as illustrated in Figure 6b.
In the case of a cantilever beam with a SiO2 layer, the cantilever beam experiences a shear force F0 to counterbalance the stress caused by the SiO2 layer, as depicted in Figure 7a. As the shear force F0 is an eccentric force, it induces a stress gradient within the cantilever beam, restraining the beam’s lateral contraction. Consequently, when the SiO2 layer is released, the influence of the shear force F0 on the cantilever beam is also eliminated, removing the lateral deformation constraint within the beam. As a result, the beam undergoes lateral deformation with shortening ΔlSi, while the stress gradient generates a moment, leading to longitudinal bending deformation y2, as illustrated in Figure 7b.
According to the above analysis, considering the compressive stress provided by the SiO2 layer in the SOI wafer needs to be shared by the substrate layer and the device layer. That is to say, the value of the residual stress in the SiO2 layer has a residual stress value that is the sum of the substrate layer and the device layer, so the amount of deformation that occurs when removing the SiO2 layer will be greater than the amount of deformation that occurs when removing the substrate layer. Therefore, in the actual process of the MEMS beam, due to the residual stress existing in the SOI wafer, after releasing the substrate and the SiO2 layer, the cantilever beam not only shortens laterally but also deflects downward. By establishing the mechanical relationship between residual stress and residual strain of MEMS beams, residual stress in SOI wafers can be better mapped. The schematic diagram of SOI cantilever beam deformation after two different processes is shown in Figure 8.
First, to examine the impact of shear force F0 on the SiO2 layer of the cantilever beam, a SiO2 sacrificial layer is incorporated into the downward curved cantilever beam. This addition serves two purposes: it not only induces lateral elongation ΔlSi but also generates deflection deformation in the cantilever beam, as illustrated in Figure 9. Specifically, the addition of the SiO2 layer can be regarded as applying a bending moment M0 to the cantilever beam, thereby altering the deflection of the beam from downward to upward. Consequently, the resulting deflection is manifested as y1 and y2.
The relationship between equivalent moment M0 and the shear force F0 can be expressed as
M 0 = F 0 × h 2
where h represents the thickness of the cantilever beam. The deflection y and angle θ of the cantilever beam caused by the bending moment M0 are, respectively, expressed as
y = M 0 l 2 2 E I
θ = M 0 l   2 E I
where l represents the length and I denote the moment of inertia of the cantilever beam. E corresponds to the elastic modulus of the material used for the cantilever beam. When subjected to the shear force F0, the cantilever beam experiences a stretching effect, resulting in an elongation ΔlSi in its length.
Δ l S i   = F 0 l   E A
where A represents the cross-sectional area of the cantilever beam.
The effect of shear force F1 from the substrate on the cantilever beam with a SiO2 layer can be analyzed. When subjected to shear force F1, the cantilever beam with a SiO2 layer experiences two distinct responses. First, it undergoes lateral shrinkage denoted as   Δ l S i O 2 . Additionally, it undergoes deflection deformation, as illustrated in Figure 10. This deflection deformation can be understood as the application of a bending moment M1 to the beam structure. As a result, the beam’s deflection changes from an upward direction to a horizontal state, resulting in a deflection of −y1.
The relationship between the equivalent moment M1 and the shear force F1 can be expressed as
M 1 = F 1 × h 2
where h′ represents the thickness of the silicon dioxide layer. The deflection y1 and angle θ1 of the beam structure caused by the bending moment M1 are, respectively, expressed as
y 1 = M 1 l 2 2 E ¯ I ¯
θ 1 = M 1 l 2 E ¯ I ¯
where E ¯ I ¯ is the equivalent bending stiffness of the composite beam. The shrinkage length   Δ l S i O 2 of the silicon dioxide layer due to the shear force F1 is
Δ l S i O 2 = F 1 l E A
where E′ represents the elastic modulus of silicon dioxide and A′ represents the cross-sectional area of silicon dioxide layer.
Clearly, under the constraint of the substrate and silicon dioxide layer, the cantilever beam top silicon layer can be reverted to a horizontal state from downward deflection, which is equivalent to applying a bending moment M2 to the cantilever beam, and the resulting deflection is y2, as shown in Figure 11.
The deflection y2 and angle θ2 of the cantilever beam caused by the bending moment M2 are, respectively, expressed as
y 2 = M 2 l 2 2 E I
θ 2 = M 2 l E I
The deformation of the cantilever beam, characterized by downward deflection and lateral shortening, is illustrated in Figure 12. By incorporating the mechanical deformation analysis of the cantilever beam, the lateral contraction length ΔlSi and the deflection y2 of the beam structure can be represented as Δ l 1 and d 1 , respectively.
Δ l 1 = Δ l s i
d 1 = y 2
The bending deformation exhibited by the cantilever beam is attributed to its internal residual stresses. As a result, it is assumed that no deformation occurs at the free end of the cantilever beam. Instead, the resulting deformation is compensated by the application of a reverse axial force F B and a bending moment M B .This arrangement forms an equivalent system for the original static indeterminate beam, as depicted in Figure 13.
In the equivalent system of statically indeterminate beams, the axial tensile length Δl2 caused by axial force FB, and the deflection f2 caused by bending moment MB are, respectively, expressed as
Δ l 2 = F B l E A
d 2 = M B l 2 2 E I
The axial tensile length Δl and the deflection f of the cantilever beam are
Δ l = Δ l 1 + Δ l 2 = Δ l s i + F B l E A
d = d 1 + d 2 = y 2 + M B l 2 2 E I
The total length of the beam does not change and the deflection and deflection angle at the right end of the beam structure is zero. Therefore, the corresponding deformation coordination conditions are
Δ l = 0 d = 0
By substituting from Equations (15) and (16) into Equation (17), FB and MB can be obtained as
F B = E A Δ l s i l
M B = 2 E I × y 2 l 2
From the axial force FB and bending moment MB, the residual stress σ can be derived as
y = y 1 + y 2
σ = F B A + M B × y I z
where y represents the distance from any point to the neutral axis.
The approach allows for the conversion of the residual stress induced by deformation at the free end of the cantilever beam into an expression that relates to the axial force and bending moment at the right end of the beam. This establishes a mechanical theoretical model for the residual stress in SOI wafers, which is mapped by the residual strain of MEMS beams. By measuring the bending moment of the MEMS beams at various points during the machining process, the beam’s deformation deflection and deflection angle can be determined at each moment. The residual stress value within the cantilever beam is then linked to the equivalent values of axial restraint and bending moment. Through the measurement of axial restraint and bending moment, it becomes possible to obtain the residual stress present within the SOI chip.

4. Experimental Test and Result Analysis

4.1. Sample Preparation and Experimental Test

In the experiment, two SOI wafers with both wafer orientations <100> are utilized to fabricate cantilever beam samples. Each SOI wafer consists of a 6 μm top silicon device layer, a 1 μm SiO2 layer, and a 380 μm silicon substrate. The Young’s modulus of the SiO2 layer as a thin-film material decreases with increasing thickness, and its corresponding Young’s modulus is 88 GPa, 81 GPa, and 77 GPa for SiO2 layer thicknesses of 0.5 μm, 1 μm, and 2 μm, respectively [30]. In this work, the thickness of the SiO2 layer is 1 μm and Young’s modulus is defined as 81 GPa.
The preparation process for the cantilever beam samples is outlined in Figure 14. For SOI wafer 1, the substrate and SiO2 layer of the cantilever beam are removed. This results in a cantilever beam structure with only the top silicon device layer remaining. For SOI wafer 2, the substrate is removed while the SiO2 layer is retained. The cantilever beam structure of this wafer consists of the top silicon device layer and the SiO2 layer, with the substrate removed.
In the experiment, a confocal laser scanning microscope (CLSM), as depicted in Figure 15, is employed for a deformation scanning of the samples. The scanning device has a horizontal resolution of 0.12 μm and a Z-axis resolution of 0.01 μm. Figure 16 illustrates the images of two types of cantilever beams: one with the removal of the SiO2 layer and the other without such removal. Both types of cantilever beams exhibit significant residual deformation at the tail end. This residual deformation is characterized by out-of-plane deflection, which leads to blurriness or incompleteness when observed under an optical microscope. To address this, the residual stress of the wafer is characterized and analyzed based on the strain measured from the cantilever beam. The specific process for characterization is outlined in Figure 17.

4.2. The Result Analysis

In the experiment, two sets of cantilever beams with the same position coordinates are tested on two SOI wafers. In the first group, there are two types of cantilever beams. The first type, referred to as CNT-1, does not have the SiO2 layer and has a length of 2000 μm and a width of 18 μm. The second type, denoted as CNT-2, has the SiO2 layer intact and has a length of 2000 μm and a width of 18 μm. In the second group, there are also two types of cantilever beams. The first type, labeled as CNT-3, does not have the SiO2 layer and has a length of 2000 μm and a width of 14 μm. The second type, designated as CNT4, has the SiO2 layer and has a length of 2000 μm and a width of 14 μm. However, it is worth noting that CNT-4 has experienced fracture at the midpoint, resulting in a remaining beam length of approximately 1000 μm. The structural morphology of the first group of cantilever beams (CNT-1 and CNT-2) has been obtained through CLSM, as depicted in Figure 18.
The residual strain data of the cantilever beams were obtained through experimental measurements, and curve fitting was performed using MATLAB. The deformation curves for the first and second groups of cantilever beams are depicted in Figure 19 and Figure 20, respectively.
Considering that the length of the cantilever beam is 2000 μm, any data beyond this range are considered invalid in Figure 19. In Figure 19a, the deformation curve of the CNT-1 cantilever beam is presented. When the substrate and the SiO2 layers are removed, the cantilever beam exhibits a downward deflection deformation. This deflection direction aligns with the predictions of the mechanical theoretical model discussed earlier, with a deflection magnitude of 28.8 μm. The roughness present in the curve mainly stems from the surface roughness of the beam after the SiO2 layer removal. Figure 19b illustrates the deformation curve of the CNT-2 cantilever beam. It can be observed that the cantilever beam, with the SiO2 layer intact, undergoes an upward deflection deformation. This deflection direction also aligns with the predictions of the mechanical theoretical model, resulting in a deflection of 307.7 μm.
In Figure 20a, the deformation curve of the CNT-3 cantilever beam is presented, exhibiting a downward deflection of 15.14 μm. In Figure 20b, the deformation curve of the CNT-4 cantilever beam is displayed. However, due to the cantilever beam fracture occurring at 1000 μm, data beyond this point are considered invalid. Within the valid data range, the cantilever beam, with the SiO2 layer intact, undergoes an upward deflection deformation with a deflection of 80.8 μm.
For the first group of cantilever beams, CNT-1 and CNT-2, the residual stress of the cantilever beam is calculated by combining the experimentally measured residual strain data with the mechanical theoretical model. The relevant mechanical results are summarized in Table 1. Similarly, the residual stress of the second group of cantilever beams is calculated using the same method, and the mechanical parameters’ results are presented in Table 2.
Based on the calculation results mentioned above, the residual stress in the SOI wafer, determined by mapping the residual strain of the two sets of MEMS beams, is found to be 33.03 MPa and 31.45 MPa, respectively. Sasaki et al. [21] established a mechanical model to map residual stresses by utilizing the rotational deformation of a ring frame. They measured the rotational deformation of the ring support frame using a white light interferometer to characterize the residual stresses in SOI wafers, yielding values of approximately 47 MPa. Zhang et al. [22] employed a micro-pointer indication structure to characterize residual stress in a fixed-supported beam structure. The residual stress in the measured structure was deduced from the deflection of the rotating beam caused by the residual stress in the fixed-supported beam structure. They characterized the residual stress in the SOI wafer to be approximately 25 MPa. The values of residual stresses calculated in this paper are in the same order of magnitude and close to those reported in the literature, indicating the feasibility of the proposed method. In addition, compared with other research results, the method proposed in this paper has higher numerical accuracy, and the absolute value of the two sets of measured values is 1.58 MPa, which makes the numerical reference more accurate.
The agreement between the calculated residual stress and the measured residual strain of the cantilever beam in this paper further validates the accuracy and feasibility of the proposed residual stress characterization method for SOI wafers.
The method proposed in this paper for measuring SOI residual stress primarily relies on stable and effective mechanical theoretical models and formulas. Moreover, since the method only requires measuring the residual strain of the cantilever beam, the testing process is simplified, resulting in higher efficiency, lower cost, and easier operation.
In industrial production, the characterization of residual stress in SOI wafers is often challenging. However, the theory proposed in this paper provides a more precise range for determining the value of residual stress, thus offering valuable insights for industrial manufacturing.

5. Conclusions

Due to the inconsistent material properties of silicon and silicon dioxide, thermal mismatch stress and intrinsic stress occur when a thin layer of silicon dioxide grows on the silicon surface. The presence of residual stress affects the performance of MEMS devices fabricated using SOI silicon wafers. In this paper, we propose a high-precision, easy-to-implement, and cost-effective characterization method for measuring residual stress in SOI wafers. We analyze the generation mechanism of residual stress in SOI wafers and develop a mechanical theoretical model for MEMS beams. The feasibility of our method is verified through experimental testing and characterization using laser scanning confocal microscopy. This research provides theoretical references and experimental support for the design and optimization of devices based on SOI-MEMS technology.

Author Contributions

Conceptualization, methodology and writing—original draft preparation, H.Y.; validation, investigation and writing—review and editing, M.L.; resources, Y.Z.; supervision and formal analysis, W.W.; visualization, X.Q.; data curation, L.H.; project administration, K.J. All authors have read and agreed to the published version of the manuscript.

Funding

This research was funded by [National Key Research and Development Program] grant number [Grant No. 2022YFB3204800]. The [Youth Innovation Team of Shaanxi Universities] [Grant No. 2022-63], and the [Key Research and Development Program of Shaanxi] [Program No. 2022NY-211].

Data Availability Statement

No new data were created for this work.

Acknowledgments

This work is sponsored by the National Key Research and Development Program [Grant No. 2022YFB3204800], the Youth Innovation Team of Shaanxi Universities [Grant No. 2022-63], and the Key Research and Development Program of Shaanxi [Program No. 2022NY-211].

Conflicts of Interest

The authors declare no conflict of interest.

References

  1. Tsou, C.; Fang, W. The effect of residual stresses on the deformation of semi-circular micromachined beams. J. Micromech. Microeng. 1999, 10, 34. [Google Scholar] [CrossRef]
  2. Jia, J.Y.; Tian, W.C. Membrane Stress Study of Micro-electromechanical System. Chin. J. Sci. Instrum. 2003, S1, 2–3. [Google Scholar]
  3. Guo, C.Q.; Pei, Z.L.; Fan, D.; Liu, R.D.; Gong, J.; Sun, C. Predicting multilayer film’s residual stress from its monolayers. Mater. Des. 2016, 110, 858–864. [Google Scholar] [CrossRef]
  4. Qian, J.; Liu, C.; Zhang, D.C.; Zhao, Y.P. Residual stresses in micro-electro-mechanical systems. J. Mech. Strength 2001, 23, 393–401. [Google Scholar]
  5. Chen, K.S.; Ou, K.S. Modification of curvature-based thin-film residual stress measurement for MEMS applications. J. Micromech. Microeng. 2002, 12, 917–924. [Google Scholar] [CrossRef]
  6. Tiberj, A.; Fraisse, B.; Blanc, C.; Contreras, S.; Camassel, J. Process-induced strain in silicon-on-insulator materials. J. Phys. Condens. Matter 2002, 14, 13411. [Google Scholar] [CrossRef]
  7. Bera, T.; Thakur, A.D. Determination of residual stress in MEMS cantilevers. AIP Conf. Proc. 2014, 1591, 683–684. [Google Scholar]
  8. Lin, C.Y.; Dai, C.L. Manufacture of Radio Frequency Micromachined Switches with Annealing. Sensors 2014, 14, 1680–1690. [Google Scholar] [CrossRef] [Green Version]
  9. Boominathasellarajan, S.; Saravanan, P.; Pandey, K.K.; Srihari, V.; Poswal, H.K. Study on the influence of residual stress on the mechanical characteristics of free-standing Si-membranes processed by deep reactive ion etching. Sens. Actuators A Phys. 2019, 290, 71–79. [Google Scholar] [CrossRef]
  10. Nelson, D.V.; Mccrickerd, J.T. Residual-stress determination through combined use of holographic interferometry and blind-hole drilling. Exp. Mech. 1986, 26, 371–378. [Google Scholar] [CrossRef]
  11. Steinzig, M.; Ponslet, E. Residual Stress Measurement Using the Hole Drilling Method and Laser Speckle Interferometry: Part 1. Exp. Tech. 2003, 27, 43–46. [Google Scholar] [CrossRef]
  12. Schajer, G.S.; Rickert, T.J. Incremental Computation Technique for Residual Stress Calculations Using the Integral Method. Exp. Mech. 2011, 51, 1217–1222. [Google Scholar] [CrossRef]
  13. Suterio, R.; Albertazzi, A.; Amaral, F.K. Residual stress measurement using indentation and a radial electronic speckle pattern interferometer—Recent progress. J. Strain Anal. 2006, 41, 517–524. [Google Scholar] [CrossRef]
  14. Mcginnis, M.J.; Pessiki, S.; Turker, H. Application of three-dimensional digital image correlation to the core-drilling method. Exp. Mech. 2005, 45, 359. [Google Scholar] [CrossRef]
  15. Min, Y.; Hong, M.; Xi, Z.; Jian, L. Determination of residual stress by use of phase shifting moire interferometry and hole-drilling method. Opt. Lasers Eng. 2006, 44, 68–79. [Google Scholar] [CrossRef]
  16. Nelson, D.V.; Makino, A.; Schmidt, T. Residual Stress Determination Using Hole Drilling and 3D Image Correlation. Exp. Mech. 2006, 46, 31–38. [Google Scholar] [CrossRef]
  17. Jiang, H.; Zhou, M.L.; Lu, J. A Computational Method of Residual Stress Calculation for Incremental Hole-Drilling Method Utilized Composite Materials. Mater. Sci. Forum 2015, 813, 94–101. [Google Scholar] [CrossRef]
  18. Dobročka, E.; Novák, P.; Búc, D.; Harmatha, L.; Murín, J. X-ray diffraction analysis of residual stresses in textured ZnO thin films. Appl. Surf. Sci. 2017, 395, 16–23. [Google Scholar] [CrossRef]
  19. Fu, X.; Niu, Z.; Deng, Y.; Zhang, J.; Liu, C.; Chen, G.; Li, Z.; Zhou, W. Accuracy of X-ray diffraction measurement of residual stresses in shot peened titanium alloy samples. Nondestruct. Test. Eval. 2019, 34, 164–177. [Google Scholar] [CrossRef]
  20. Zhu, L.-N.; Xu, B.-S.; Wang, H.-D.; Wang, C.-B. Microstructure and nanoindentation measurement of residual stress in Fe-based coating by laser cladding. J. Mater. Sci. 2012, 47, 2122–2126. [Google Scholar] [CrossRef]
  21. Sasaki, T.; Hane, K. Deformation of varifocal mirror with narrow frame by SOI wafer residual stress. Electron. Commun. Jpn. 2012, 95, 26–33. [Google Scholar] [CrossRef]
  22. Zhang, X.; Zhang, T.Y.; Zohar, Y. Measurements of residual stresses in thin films using micro-rotating-structures. Thin Solid Film. 1998, 335, 97–105. [Google Scholar] [CrossRef]
  23. Suresh, S.; Giannakopoulos, A.E. A new method for estimating residual stresses by instrumented sharp indentation. Acta Mater. 1998, 46, 5755–5767. [Google Scholar] [CrossRef]
  24. Lee, Y.-H.; Kwon, D. Residual stresses in DLC/Si and Au/Si systems: Application of a stress-relaxation model to the nanoindentation technique. J. Mater. Res. 2002, 17, 901–906. [Google Scholar] [CrossRef]
  25. Swadener, J.G.; Taljat, B.; Pharr, G.M. Measurement of residual stress by load and depth sensing indentation with spherical indenters. J. Mater. Res. 2001, 16, 2091–2102. [Google Scholar] [CrossRef]
  26. Xu, Z.-H.; Li, X. Influence of equi-biaxial residual stress on unloading behaviour of nanoindentation. Acta Mater. 2005, 53, 1913–1919. [Google Scholar] [CrossRef]
  27. Chung, G.S.; Choi, S.K.; Nam, H.D. Design, fabrication, and characteristics of microheaters with low consumption power using SDB SOI membrane and trench structures. Micromach. Microfabr. Process Technol. Devices 2001, 4601, 346–353. [Google Scholar]
  28. Mäkinen, J.; Suni, T. Thick-film SOI wafers: Preparation and properties. In Handbook of Silicon Based MEMS Materials and Technologies; William Andrew Publishing: Norwich, NY, USA, 2015; pp. 206–237. [Google Scholar]
  29. Datta, R.; Allen, L.P.; Dolan, R.P.; Jones, K.S.; Farley, M. Independent implant parameter effects on SIMOX SOI dislocation formation. Mater. Sci. Eng. B 1997, 46, 8–13. [Google Scholar] [CrossRef]
  30. Nie, X.; Li, J.; Lang, F. Effect of Film Thickness on Mechanical Properties of Si-based SiO2 Thin Films. Mech. Sci. Technol. Aerosp. Eng. 2019, 38, 646–651. [Google Scholar]
Figure 1. The process of SDB technology for preparing SOI wafers.
Figure 1. The process of SDB technology for preparing SOI wafers.
Micromachines 14 01510 g001
Figure 2. Edge mismatch dislocation due to lattice mismatch.
Figure 2. Edge mismatch dislocation due to lattice mismatch.
Micromachines 14 01510 g002
Figure 3. The residual stress distribution of the layer and substrate (edges).
Figure 3. The residual stress distribution of the layer and substrate (edges).
Micromachines 14 01510 g003
Figure 4. Distribution of residual stress in an SOI wafer (edges).
Figure 4. Distribution of residual stress in an SOI wafer (edges).
Micromachines 14 01510 g004
Figure 5. (a) The ideal state of a cantilever beam. (b) The schematic diagram of gradient stress.
Figure 5. (a) The ideal state of a cantilever beam. (b) The schematic diagram of gradient stress.
Micromachines 14 01510 g005
Figure 6. (a) The shear force of substrate on the silicon layer. (b) The deformation of a cantilever beam with a SiO2 layer after releasing substrate.
Figure 6. (a) The shear force of substrate on the silicon layer. (b) The deformation of a cantilever beam with a SiO2 layer after releasing substrate.
Micromachines 14 01510 g006
Figure 7. (a) The shear force of the SiO2 layer on the cantilever beam. (b) The deformation of the cantilever beam after releasing the SiO2 layer.
Figure 7. (a) The shear force of the SiO2 layer on the cantilever beam. (b) The deformation of the cantilever beam after releasing the SiO2 layer.
Micromachines 14 01510 g007
Figure 8. SOI cantilever beam deformation diagram.
Figure 8. SOI cantilever beam deformation diagram.
Micromachines 14 01510 g008
Figure 9. The effect of a silicon dioxide layer on the cantilever beam.
Figure 9. The effect of a silicon dioxide layer on the cantilever beam.
Micromachines 14 01510 g009
Figure 10. The effect of substrate on the composite beam.
Figure 10. The effect of substrate on the composite beam.
Micromachines 14 01510 g010
Figure 11. The effect of substrate and silicon dioxide on the cantilever beam.
Figure 11. The effect of substrate and silicon dioxide on the cantilever beam.
Micromachines 14 01510 g011
Figure 12. Deformation analysis of the cantilever beam.
Figure 12. Deformation analysis of the cantilever beam.
Micromachines 14 01510 g012
Figure 13. The equivalent system of the statically indeterminate beam.
Figure 13. The equivalent system of the statically indeterminate beam.
Micromachines 14 01510 g013
Figure 14. Schematic diagram of the preparation process for two SOI wafers.
Figure 14. Schematic diagram of the preparation process for two SOI wafers.
Micromachines 14 01510 g014
Figure 15. Physical image of confocal laser scanning microscope.
Figure 15. Physical image of confocal laser scanning microscope.
Micromachines 14 01510 g015
Figure 16. Images of two types of cantilever beams: (a) transverse cantilever beam (no sacrifice layer released), (b) longitudinal cantilever beam (no sacrifice layer released), (c) transverse cantilever beam (sacrificial layer released), and (d) longitudinal cantilever beam (sacrificial layer released).
Figure 16. Images of two types of cantilever beams: (a) transverse cantilever beam (no sacrifice layer released), (b) longitudinal cantilever beam (no sacrifice layer released), (c) transverse cantilever beam (sacrificial layer released), and (d) longitudinal cantilever beam (sacrificial layer released).
Micromachines 14 01510 g016
Figure 17. Schematic diagram of residual stress characterization process.
Figure 17. Schematic diagram of residual stress characterization process.
Micromachines 14 01510 g017
Figure 18. The 3D morphology of the first group of cantilever beams: (a) CNT-1 and (b) CNT-2.
Figure 18. The 3D morphology of the first group of cantilever beams: (a) CNT-1 and (b) CNT-2.
Micromachines 14 01510 g018
Figure 19. Beam deformation curves of the first group of cantilever beams: (a) CNT-1 and (b) CNT-2.
Figure 19. Beam deformation curves of the first group of cantilever beams: (a) CNT-1 and (b) CNT-2.
Micromachines 14 01510 g019
Figure 20. Beam deformation curves of the second group of cantilever beams: (a) CNT-3 and (b) CNT-4.
Figure 20. Beam deformation curves of the second group of cantilever beams: (a) CNT-3 and (b) CNT-4.
Micromachines 14 01510 g020
Table 1. The mechanical parameters’ results of the first group cantilever beams.
Table 1. The mechanical parameters’ results of the first group cantilever beams.
Mechanical ParametersSymbolValue
Deflection of composite cantilever beamy1307.7 μm
Deflection of cantilever beamy228.8 μm
Shortened length of cantilever beamΔlSi0.337 μm
Restrained axial force of clamped beamFB28.39 N
Restrained bending moment of clamped beamMB7.28 × 10−10 N·m
Residual stressσ33.03 MPa
Table 2. The mechanical parameters’ results of the second group cantilever beams.
Table 2. The mechanical parameters’ results of the second group cantilever beams.
Mechanical ParametersSymbolValue
Deflection of composite cantilever beam y180.08 μm
Deflection of cantilever beam y210.1 μm
Shortened length of cantilever beam ΔlSi0.141 μm
Restrained axial force of clamped beamFB18.48 N
Restrained bending moment of clamped beamMB7.94 × 10−10 N·m
Residual stressσ31.45 MPa
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content.

Share and Cite

MDPI and ACS Style

Yang, H.; Liu, M.; Zhu, Y.; Wang, W.; Qin, X.; He, L.; Jiang, K. Characterization of Residual Stress in SOI Wafers by Using MEMS Cantilever Beams. Micromachines 2023, 14, 1510. https://doi.org/10.3390/mi14081510

AMA Style

Yang H, Liu M, Zhu Y, Wang W, Qin X, He L, Jiang K. Characterization of Residual Stress in SOI Wafers by Using MEMS Cantilever Beams. Micromachines. 2023; 14(8):1510. https://doi.org/10.3390/mi14081510

Chicago/Turabian Style

Yang, Haotian, Min Liu, Yingmin Zhu, Weidong Wang, Xianming Qin, Lilong He, and Kyle Jiang. 2023. "Characterization of Residual Stress in SOI Wafers by Using MEMS Cantilever Beams" Micromachines 14, no. 8: 1510. https://doi.org/10.3390/mi14081510

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.