Effect of Substrate-RF on Sub-200 nm Al0.7Sc0.3N Thin Films
 
 
Font Type:
Arial Georgia Verdana
Font Size:
Aa Aa Aa
Line Spacing:
Column Width:
Background:
Article

High-Temperature Ferroelectric Behavior of Al0.7Sc0.3N

1
Colorado School of Mines, 1500 Illinois Ave., Golden, CO 80401, USA
2
National Renewable Energy Laboratory, 15013 Denver West Parkway, Golden, CO 80401, USA
3
U.S. Army Combat Capabilities Development Command—Army Research Laboratory, Adelphi, MD 20783, USA
*
Authors to whom correspondence should be addressed.
Micromachines 2022, 13(6), 887; https://doi.org/10.3390/mi13060887
Submission received: 12 May 2022 / Revised: 30 May 2022 / Accepted: 30 May 2022 / Published: 31 May 2022

Abstract

:
Currently, there is a lack of nonvolatile memory (NVM) technology that can operate continuously at temperatures > 200 °C. While ferroelectric NVM has previously demonstrated long polarization retention and >1013 read/write cycles at room temperature, the largest hurdle comes at higher temperatures for conventional perovskite ferroelectrics. Here, we demonstrate how AlScN can enable high-temperature (>200 °C) nonvolatile memory. The c-axis textured thin films were prepared via reactive radiofrequency magnetron sputtering onto a highly textured Pt (111) surface. Photolithographically defined Pt top electrodes completed the capacitor stack, which was tested in a high temperature vacuum probe station up to 400 °C. Polarization–electric field hysteresis loops between 23 and 400 °C reveal minimal changes in the remanent polarization values, while the coercive field decreased from 4.3 MV/cm to 2.6 MV/cm. Even at 400 °C, the polarization retention exhibited negligible loss for up to 1000 s, demonstrating promise for potential nonvolatile memory capable of high−temperature operation. Fatigue behavior also showed a moderate dependence on operating temperature, but the mechanisms of degradation require additional study.

1. Introduction

Nonvolatile memories, which do not require a permanent/frequent voltage supplied to maintain the bit state, are important for storing information indefinitely and reliably. The concept of high−operating−temperature nonvolatile memory (HOT−NVM) has been an elusive capability. Current computational and data storage limitations in harsh environments either require on−board cooling or locating sensors/computations away from the heat source. These harsh environments for electronics are a focus of the NASA HOTTech project and can be found within jet turbines, within deep−well drilling, and on the surface of Venus [1].
Nonvolatile random−access memory (RAM) based on FLASH, magnetic, phase−change, and resistive mechanisms degrade quickly even at moderate temperatures (<200 °C) [2,3,4,5]. Microelectromechanical (MEM) and nanogap resistance switching (NGS) offer promise for elevated temperatures NVM, but there are downsides with moving parts and operating in various atmospheres [6,7]. Ferroelectric technology based on perovskite or fluorite structures (e.g., Pb(Zr,Ti)O3 or (Hf,Zr,Si)O2) is currently limited to temperatures < 200 °C [8,9]. This is a result of a destabilized polar structure, chemical instabilities, and increased domain wall mobility in Pb(Zr,Ti)O3 [10,11], whereas increased pyroelectric contributions and depolarization fields plague (Hf,Zr)O2 compositions when increasing temperature [12,13]. Here, we demonstrate promising initial results when using ferroelectric Al0.7Sc0.3N to meet the HOT−NVM demands.
Since its discovery in 2019 as the first wurtzite nitride ferroelectric, Al1xScxN (AlScN) has received much attention from both the ferroelectric and piezoelectric communities [14]. The high remanent polarization (Pr) associated with the ideal wurtzite structure is an attractive property for increasing either device density or extracted charge density. Previous studies on AlN−based ferroelectrics reported the high coercive field (Ec) necessary to switch between the two polarization states. While this high Ec is problematic for integration with low−voltage devices, it can be valuable for retention characteristics as temperatures increase [8]. The Ec of AlScN can be tuned through various modifications such as composition [14,15,16], stress [17], epitaxial alignment [18], and temperature [19,20,21,22]. In addition to thickness scaling, these trends are important for integrating AlScN into a high−temperature chip to reduce the operating voltages.
To assess polarization stability for a nonvolatile memory, Islam et al. poled the sample at room temperature (RT), baked the package at 1100 °C, and remeasured the Pr once cooled back to RT [23]. While promising for an NVM since the polarization state is maintained after exposure to extreme temperatures, these ex situ results did not address the Pr or switching behavior at elevated temperatures. Liu et al. focused on the retention state at RT for an AlScN ferroelectric−gated field effect transistor (FET) device by monitoring changes in the resistance state over time [24]. Furthermore, an NVM must endure switching cycles without compromising the Pr or Ec values, which can impact deciphering between either polarization state, and the device must avoid electrical shorts. Two recent reports have noted that AlScN has low endurance, a measure of repeated bit flips, at <105 cycles before dielectric failure, which may be limited by the slim margin between coercive and breakdown fields (Ebd) for the samples, but a true mechanistic understanding of fatigue in AlScN is still lacking [25,26]. Thus, these reports do not represent a fundamental limitation of the ferroelectric switching endurance. In this article, we report device relevant behavior (i.e., leakage, retention, and fatigue) between 23 and 400 °C to introduce AlScN as a candidate material for HOT−NVM.

2. Materials and Methods

The 225 nm thick ferroelectric AlScN film was deposited by radiofrequency (rf) reactive magnetron sputtering onto a highly textured Pt (111) bottom electrode. The base pressure of the chamber reached 2 × 10−6 Torr prior to flowing the deposition gases. The pressure was maintained at 2 mTorr while flowing 5 sccm N2 and 15 sccm Ar. Furthermore, 300 W of rf power was supplied to the 5 cm diameter Al0.7Sc0.3 alloy target. The substrate was heated to 400 °C and positioned 16.5 cm from the target. Details of sputter deposition processes using in situ optical emission spectrometry were previously described [27]. The target was conditioned with a 1 h pre−sputter to remove surface oxidation and stabilize the reactive target mode. Following the nitride layer deposition, lithographically defined 50 μm diameter platinum top electrodes were sputter−deposited to form a metal−ferroelectric−metal (MFM) structure for electrical testing.
The resultant AlScN film was structurally characterized by X−ray diffraction (XRD) using Cu Kα radiation. A Panalytical X’Pert MRD diffractometer was used to scan the θ−2θ and ω space. The sample was tested in a high−temperature vacuum probe station to mitigate possible oxidation of the nitride. Electrical properties of the MFM capacitors were measured using a ferroelectric analyzer (Radiant Precision Premier II).
The MFM capacitors were evaluated with DC current−voltage (IV) sweeps to assess the resistivity at various temperatures; this is important for evaluating polarization values that may be inflated by charge leakage. Polarization−electric field (P–E) hysteresis loops were collected between probe station temperatures of 23−400 °C using an excitation frequency of 10 kHz. This frequency was chosen to reduce the leakage contribution to the Pr values, and 10 kHz is a relatively high frequency when compared to previous reports on ferroelectric AlScN, which range between 333 Hz and 100 kHz [19,21]. Retention testing was used to measure the stability of a polarization state over time to inspect the volatility of that state. The test involved a positive or negative pre−pulse to the bottom electrode to pole the sample in either a metal or a nitrogen polar orientation, respectively. This was followed by a dwell for a length of time, and then the MFM capacitor was pulsed twice with the same voltage profile (Figure 1). The measured 2Pr elucidates whether the capacitor underwent ferroelectric polarization switching between pulse 1 and pulse 2 or not. In this study, four different pulse sequences were necessary to characterize the same state and opposite state retention characteristics for each polarization state—nitrogen (N) and metal (M) polar. A ‘same state’ (SS) test indicates that the bias of the read and write pulses is the same, while an ‘opposite state’ (OS) test switches pulse polarity. The difference between a switched and unswitched polarization response is 2Pr. If the 2Pr shrinks over time, then the bit state will eventually be indecipherable; therefore, a stable polarization value is essential for NVM memory applications. Ten virgin capacitors with an active (top electrode) diameter of 50 μm were assessed at each temperature. P–E loops (10 kHz) were collected prior to each 1000 cycle (1 kHz triangular waveform applied for 1 s) fatigue to inspect the ferroelectric properties throughout the process.

3. Results and Discussion

3.1. Structural and Leakage Characteristics

In Figure 2a, the XRD scan reveals a wurtzite phase of AlScN with c−axis texture. The (0002) reflection appeared at 36.056° in with a full width at half maximum (FWHM) value of 0.158°. The ω−rocking scan of the (0002) position resulted in an FWHM value of 2.694°, which is comparable to prior reports (Figure 2b) [16,22]. Lack of additional wurtzite peaks associated with other orientations indicates that the film had a purely c−axis texture. Since the c−axis is the polar axis of the wurtzite structure, it is important to maximize the degree of c−axis out of plane texture when investigating the ferroelectric properties of an MFM capacitor (inset of Figure 2a).
The P–E loops measured at 10 kHz between 23 and 400 °C reveal a strong dependence of the Ec on temperature (Figure 3a). The square−like hysteresis loops were a result of a relatively low permittivity, defined energy barriers between polarization states, and minimal loss mechanisms. Levels of polarization saturation similar to previous reports were reached at each temperature [14,16]. At 400 °C, the derivative dP/dE became negative after saturation, indicating decreased capacitor resistance. This observation is supported by the current density–electric field (J–E) sweeps in Figure 3b. When subjected to a 1 MV·cm−1 DC field, the current density rose from 1 × 10−7 A·cm−2 at 23 °C to 3 × 10−4 A·cm−2 at 400 °C. Furthermore, J increased exponentially with E and maintained this relationship at all temperatures. The increasing leakage with temperature is important for compensation when possibly measuring changes in polarization (e.g., during retention testing).
The ΔEc/2 decreased linearly as temperature increased, describing a reduced activation barrier due to thermal energy contribution. An Ec temperature coefficient of 4.5 kV·cm−1·K−1 describes our results in Figure 3c, which showed a decrease from 4.3 to 2.6 MV·cm−1 between 23 and 400 °C. In the limited number of reports that analyzed the Ec and Pr dependence on temperature for Al1−xScxN, there were a range of compositions studied with various frequencies. Our data (30% Sc, 10 kHz) showed a slightly lower Ec temperature coefficient in comparison to the literature. The overall Ec results (apart from the reduced Ec values reported by Wang et al.) are consistent with the literature in terms of a lower Ec due to increasing Sc content or decreasing excitation frequency. This may explain both the coincidental values between Gund et al. (30% Sc, 3 kHz) and Zhu et al. (16% Sc, 333 Hz) and the increased Ec for Mizutani et al. (20% Sc, 100 kHz) [19,20,21,22]. Our work shows that the Pr values for Al0.7Sc0.3N remained relatively stable up to 400 °C (Figure 3d). The temperature−independent Pr behavior of an Al1xScxN composition was also noted by the mentioned reports. In general, the Pr decrease with increasing x was seen in a majority of the reports [16].

3.2. Polarization Retention at Elevated Temperatures

Retention studies were carried out relative to the surface polar state, nitrogen or metal, termed SSN, SSM, OSN, and OSM. Polarization changes were investigated with durations of pulses up to 1000 s to reveal if any changes occurred. A reduction in measured polarization would indicate that an internal process occurred, reducing the net polarization via mechanisms such as back−switching, domain pinning, or phase degradation. However, our results revealed no Pr loss, indicating a kinetically stable polarization direction and a negligible change in the polarization−pinning defect environment (Figure 4). This contrasts perovskite and fluorite−based ferroelectric MFM capacitors, which showed a clear reduction in Pr when subjected to a bake between the write and read voltage pulses [9,12,28]. For both SS tests, there was a marginal level of polarization (<6 μC·cm−2), which may have been the effect of changes in the leakage contribution between the first and second read pulses. Since the OS and SS tests for the metal and nitrogen poled devices showed a steady polarization retention between 1 and 1000 s, the estimated time until the 2Pr was reduced enough for the bit state to become indecipherable requires further retention testing before a reasonable estimate can be established. Our results are also in agreement with the RT retention tests performed by Fichtner et al., who reported steady retention up to 105 s [14]. Overall, the ferroelectric AlScN retained all the polarization that was written into the MFM capacitor, even while operating at 400 °C. This characteristic is a promising factor for enabling high−temperature nonvolatile memory.

3.3. Device Fatigue at Elevated Temperatures

To ascertain the switching endurance of the sample, 10 MFM capacitors from the same sample were tested at each temperature. The maximum field applied during the fatigue cycles and P–E loop measurements was scaled to 105% of the Ec. Figure 5a provides a summary of the fatigue results, which were also temperature−dependent. A P–E loop measurement followed every 1000 cycles to track the changes in the polarization throughout the fatigue subjection. One standard deviation is denoted by the error bars in Figure 5a. Device failure was defined at the point when the device shorted. The highest average endurance occurred at 200 °C (2.7 × 105 ± 1.9 × 105 cycles) with a maximum of 6.0 × 105 cycles. While this is an increased fatigue endurance relative to previous reports on AlScN, it still indicates that effort is needed to increase the margin between Ec and Ebd and to investigate and mitigate the underlying causes of fatigue in these materials. Because Ec decreased with increased temperature faster than Ebd decreased, the increased margin between the two was presumably an important contributor to the increase in fatigue life from RT to 200 °C. The degraded performance at temperatures > 200 °C, however, was associated with larger leakage currents in the MFM capacitor that occurred during each fatigue cycle.
The least change in polarization versus cycling happened at 100 °C. Figure 5b–f are representative snapshots of the P–E loop measured after the given number of cycles. Especially for the higher−temperature panels, the initially square−like hysteresis loops deteriorated into a combination of lower Pr and inflated polarization values due to an uncompensated leakage contribution. Additional study into the cycle−dependent leakage characteristics may point toward a specific leakage mechanism that increases in effect with cycling. Furthermore, a systematic investigation on the AlScN switching fatigue behavior for various electrode types will be critical for applications that require more resilient endurance.

4. Conclusions

In summary, a thin film, c−axis textured AlScN was electrically tested in a metal–ferroelectric–metal capacitor for polarization hysteresis, retention, and fatigue up to 400 °C. The leakage current density increased by four orders of magnitude between RT and 400 °C, which revealed the importance of compensating for the leakage contribution to polarization, especially as temperature increased. While a strong Ec dependence on temperature (4.5 kV·cm−1·K−1) led to a 60% reduction at 400 °C compared to RT, the Pr remained stable over all temperatures. As an important characteristic for NVM, in situ polarization retention testing up to 1000 s revealed negligible (<2%) polarization loss for either the metal or the nitrogen polar state at all temperatures tested up to 400 °C. On average, the highest endurance before complete failure occurred at 200 °C with 2.7 × 105 switching cycles; however, the reduction in Pr versus cycles was lowest at 100 °C. Our results showing >105 switching cycles are encouraging for using ferroelectric AlScN in HOT−NVM applications where <103 switching cycles would be required. Future work on the fatigue mechanisms at different temperatures and expanding the retention duration time are vital avenues for understanding the intrinsic limitations of AlScN.

Author Contributions

Conceptualization, D.D., B.H. and G.B.; methodology, D.D.; validation, D.D., B.H. and G.B.; formal analysis, D.D.; investigation, D.D.; resources, K.Y., A.Z. and B.H.; data curation, D.D.; writing—original draft preparation, D.D., B.H. and G.B.; writing—review and editing, D.D., B.H. and G.B.; supervision, K.Y., A.Z., B.H. and G.B.; project administration; funding acquisition, A.Z., B.H. and G.B. All authors read and agreed to the published version of the manuscript.

Funding

This research was sponsored by the Army Research Laboratory and was accomplished under Cooperative Agreement Number W911NF-21-2-0210. The views and conclusions contained in this document are those of the authors and should not be interpreted as representing the official policies, either expressed or implied, of the Army Research Laboratory or the US Government. The US Government is authorized to reproduce and distribute reprints for Government purposes notwithstanding any copyright notation herein. This work was coauthored by the Colorado School of Mines and the National Renewable Energy Laboratory, operated by the Alliance for Sustainable Energy, LLC, for the US Department of Energy (DOE) under Contract No. DE-AC36-08GO28308. Funding was provided by the DARPA Tunable Ferroelectric Nitrides (TUFEN) program (DARPA-PA-19-04-03) as a part of Development and Exploration of Ferroelectric Nitride Semiconductors (DEFENSE) project (diffraction, microscopy, and electrical characterization), and by Office of Science (SC), Office of Basic Energy Sciences (BES) as part of the Early Career Award “Kinetic Synthesis of Metastable Nitrides” (material synthesis and in situ monitoring).

Data Availability Statement

The data that support the findings of this study are available from the corresponding author upon reasonable request.

Acknowledgments

The authors also express their appreciation to Wanlin Zhu and Susan Trolier-McKinstry of the Pennsylvania State University for providing Pt/TiO2/SiO2/Si substrates. We also thank Jeff Alleman for assistance with setting up the sputter system at NREL.

Conflicts of Interest

The authors declare no conflict of interest.

References

  1. Neudeck, P.G.; Meredith, R.D.; Chen, L.; Spry, D.J.; Nakley, L.M.; Hunter, G.W. Prolonged Silicon Carbide Integrated Circuit Operation in Venus Surface Atmospheric Conditions. AIP Adv. 2016, 6, 125119. [Google Scholar] [CrossRef]
  2. Lee, K.; Kang, S.H. Design Consideration of Magnetic Tunnel Junctions for Reliable High-Temperature Operation of STT-MRAM. IEEE Trans. Magn. 2010, 46, 1537–1540. [Google Scholar] [CrossRef]
  3. Wong, H.-S.P.; Raoux, S.; Kim, S.; Liang, J.; Reifenberg, J.P.; Rajendran, B.; Asheghi, M.; Goodson, K.E. Phase Change Memory. Proc. IEEE 2010, 98, 2201–2227. [Google Scholar] [CrossRef]
  4. Ye, C.; Wu, J.; He, G.; Zhang, J.; Deng, T.; He, P.; Wang, H. Physical Mechanism and Performance Factors of Metal Oxide Based Resistive Switching Memory: A Review. J. Mater. Sci. Technol. 2016, 32, 1–11. [Google Scholar] [CrossRef]
  5. Taito, Y.; Nakano, M.; Okimoto, H.; Okada, D.; Ito, T.; Kono, T.; Noguchi, K.; Hidaka, H.; Yamauchi, T. 7.3 A 28 nm Embedded SG-MONOS Flash Macro for Automotive Achieving 200 MHz Read Operation and 2.0MB/S Write Throughput at Ti, of 170 °C. In Proceedings of the 2015 IEEE International Solid-State Circuits Conference-(ISSCC) Digest of Technical Papers, San Francisco, CA, USA, 22–26 February 2015; pp. 1–3. [Google Scholar]
  6. Suga, H.; Suzuki, H.; Shinomura, Y.; Kashiwabara, S.; Tsukagoshi, K.; Shimizu, T.; Naitoh, Y. Highly Stable, Extremely High-Temperature, Nonvolatile Memory Based on Resistance Switching in Polycrystalline Pt Nanogaps. Sci. Rep. 2016, 6, 34961. [Google Scholar] [CrossRef] [PubMed] [Green Version]
  7. Singh, P.; Arya, D.S.; Jain, U. MEM-FLASH Non-Volatile Memory Device for High-Temperature Multibit Data Storage. Appl. Phys. Lett. 2019, 115, 43501. [Google Scholar] [CrossRef]
  8. Stolichnov, I.; Tagantsev, A.K.; Colla, E.; Setter, N.; Cross, J.S. Physical Model of Retention and Temperature-Dependent Polarization Reversal in Ferroelectric Films. J. Appl. Phys. 2005, 98, 84106. [Google Scholar] [CrossRef]
  9. Mueller, S.; Muller, J.; Schroeder, U.; Mikolajick, T. Reliability Characteristics of Ferroelectric Si:HfO2 Thin Films for Memory Applications. IEEE Trans. Device Mater. Relib. 2013, 13, 93–97. [Google Scholar] [CrossRef]
  10. Kounga, A.B.; Granzow, T.; Aulbach, E.; Hinterstein, M.; Rödel, J. High-Temperature Poling of Ferroelectrics. J. Appl. Phys. 2008, 104, 24116. [Google Scholar] [CrossRef]
  11. Kamel, T.M.; Kools, F.X.N.M.; de With, G. Poling of Soft Piezoceramic PZT. J. Eur. Ceram. Soc. 2007, 27, 2471–2479. [Google Scholar] [CrossRef]
  12. Ali, T.; Kuhnel, K.; Czernohorsky, M.; Mart, C.; Rudolph, M.; Patzold, B.; Lehninger, D.; Olivo, R.; Lederer, M.; Muller, F.; et al. A Study on the Temperature-Dependent Operation of Fluorite-Structure-Based Ferroelectric HfO2 Memory FeFET: Pyroelectricity and Reliability. IEEE Trans. Electron. Devices 2020, 67, 2981–2987. [Google Scholar] [CrossRef]
  13. Mohan, J.; Hernandez-Arriaga, H.; Jung, Y.C.; Onaya, T.; Nam, C.-Y.; Tsai, E.H.R.; Kim, S.J.; Kim, J. Ferroelectric Polarization Retention with Scaling of Hf0.5Zr0.5O2 on Silicon. Appl. Phys. Lett. 2021, 118, 102903. [Google Scholar] [CrossRef]
  14. Fichtner, S.; Wolff, N.; Lofink, F.; Kienle, L.; Wagner, B. AlScN: A III-V Semiconductor Based Ferroelectric. J. Appl. Phys. 2019, 125, 114103. [Google Scholar] [CrossRef]
  15. Hayden, J.; Hossain, M.D.; Xiong, Y.; Ferri, K.; Zhu, W.; Imperatore, M.V.; Giebink, N.; Trolier-McKinstry, S.; Dabo, I.; Maria, J.-P. Ferroelectricity in Boron-Substituted Aluminum Nitride Thin Films. Phys. Rev. Mater. 2021, 5, 44412. [Google Scholar] [CrossRef]
  16. Yasuoka, S.; Shimizu, T.; Tateyama, A.; Uehara, M.; Yamada, H.; Akiyama, M.; Hiranaga, Y.; Cho, Y.; Funakubo, H. Effects of Deposition Conditions on the Ferroelectric Properties of (Al1−xScx)N Thin Films. J. Appl. Phys. 2020, 128, 114103. [Google Scholar] [CrossRef]
  17. Schönweger, G.; Petraru, A.; Islam, M.R.; Wolff, N.; Haas, B.; Hammud, A.; Koch, C.; Kienle, L.; Kohlstedt, H.; Fichtner, S. From Fully Strained to Relaxed: Epitaxial Ferroelectric Al1−xScx N for III-N Technology. Adv. Funct. Mater. 2022, 32, 2109632. [Google Scholar] [CrossRef]
  18. Yazawa, K.; Drury, D.; Zakutayev, A.; Brennecka, G.L. Reduced Coercive Field in Epitaxial Thin Film of Ferroelectric Wurtzite Al0.7Sc0.3N. Appl. Phys. Lett. 2021, 118, 162903. [Google Scholar] [CrossRef]
  19. Zhu, W.; Hayden, J.; He, F.; Yang, J.-I.; Tipsawat, P.; Hossain, M.D.; Maria, J.-P.; Trolier-McKinstry, S. Strongly Temperature Dependent Ferroelectric Switching in AlN, Al1−xScxN, and Al1−xBxN Thin Films. Appl. Phys. Lett. 2021, 119, 062901. [Google Scholar] [CrossRef]
  20. Wang, J.; Park, M.; Ansari, A. High-Temperature Acoustic and Electric Characterization of Ferroelectric Al0.7Sc0.3N Films. J. Microelectromech. Syst. 2022, 31, 234–240. [Google Scholar] [CrossRef]
  21. Mizutani, R.; Yasuoka, S.; Shiraishi, T.; Shimizu, T.; Uehara, M.; Yamada, H.; Akiyama, M.; Sakata, O.; Funakubo, H. Thickness Scaling of (Al0.8Sc0.2)N Films with Remanent Polarization beyond 100 ΜC Cm−2 around 10 Nm in Thickness. Appl. Phys. Express 2021, 14, 105501. [Google Scholar] [CrossRef]
  22. Gund, V.; Davaji, B.; Lee, H.; Asadi, M.J.; Casamento, J.; Xing, H.G.; Jena, D.; Lal, A. Temperature-Dependent Lowering of Coercive Field in 300 Nm Sputtered Ferroelectric Al0.70Sc0.30N. In Proceedings of the 2021 IEEE International Symposium on Applications of Ferroelectrics (ISAF), Sydney, Australia, 16 May 2021; pp. 1–3. [Google Scholar]
  23. Islam, M.d.R.; Wolff, N.; Yassine, M.; Schönweger, G.; Christian, B.; Kohlstedt, H.; Ambacher, O.; Lofink, F.; Kienle, L.; Fichtner, S. On the Exceptional Temperature Stability of Ferroelectric Al1-xScxN Thin Films. Appl. Phys. Lett. 2021, 118, 232905. [Google Scholar] [CrossRef]
  24. Liu, X.; Wang, D.; Kim, K.-H.; Katti, K.; Zheng, J.; Musavigharavi, P.; Miao, J.; Stach, E.A.; Olsson, R.H.; Jariwala, D. Post-CMOS Compatible Aluminum Scandium Nitride/2D Channel Ferroelectric Field-Effect-Transistor Memory. Nano Lett. 2021, 21, 3753–3761. [Google Scholar] [CrossRef] [PubMed]
  25. Mikolajick, T.; Slesazeck, S.; Mulaosmanovic, H.; Park, M.H.; Fichtner, S.; Lomenzo, P.D.; Hoffmann, M.; Schroeder, U. Next Generation Ferroelectric Materials for Semiconductor Process Integration and Their Applications. J. Appl. Phys. 2021, 129, 100901. [Google Scholar] [CrossRef]
  26. Tsai, S.-L.; Hoshii, T.; Wakabayashi, H.; Tsutsui, K.; Chung, T.-K.; Chang, E.Y.; Kakushima, K. Room-Temperature Deposition of a Poling-Free Ferroelectric AlScN Film by Reactive Sputtering. Appl. Phys. Lett. 2021, 118, 082902. [Google Scholar] [CrossRef]
  27. Drury, D.; Yazawa, K.; Mis, A.; Talley, K.; Zakutayev, A.; Brennecka, G.L. Understanding Reproducibility of Sputter-Deposited Metastable Ferroelectric Wurtzite Al0.6Sc0.4N Films Using In Situ Optical Emission Spectrometry. Phys. Status Solidi RRL 2021, 15, 2100043. [Google Scholar] [CrossRef]
  28. Rodriguez, J.A.; Remack, K.; Boku, K.; Udayakumar, K.R.; Aggarwal, S.; Summerfelt, S.R.; Celii, F.G.; Martin, S.; Hall, L.; Taylor, K.; et al. Reliability Properties of Low-Voltage Ferroelectric Capacitors and Memory Arrays. IEEE Trans. Device Mater. Relib. 2004, 4, 436–449. [Google Scholar] [CrossRef]
Figure 1. Retention test protocols for OS and SS in either a nitrogen or metal polar surface state. Green and orange traces represent switching and non−switching pulses, respectively.
Figure 1. Retention test protocols for OS and SS in either a nitrogen or metal polar surface state. Green and orange traces represent switching and non−switching pulses, respectively.
Micromachines 13 00887 g001
Figure 2. (a) The 2θ–θ XRD scan of the investigated sample revealing a pure wurtzite phase with c−axis texture. The inset depicts the stacking sequence of the metal–ferroelectric–metal capacitor. (b) ω rocking scan of the Al0.7Sc0.3N (0002) peak.
Figure 2. (a) The 2θ–θ XRD scan of the investigated sample revealing a pure wurtzite phase with c−axis texture. The inset depicts the stacking sequence of the metal–ferroelectric–metal capacitor. (b) ω rocking scan of the Al0.7Sc0.3N (0002) peak.
Micromachines 13 00887 g002
Figure 3. (a) P−E loops between 23 and 400 °C collected with 10 kHz bipolar voltage waveform. (b) Temperature−dependent leakage current density (J) over bias between 23 and 400 °C. Comparison of (c) ∆Ec/2 and (d) Pr results from this work with Mizutani et al. [21], Zhu et al. [20], Gund et al. [22], and Wang et al. [20]. The results in (a,b) are from this work, while (c,d) are a comparison of our results with previous reports.
Figure 3. (a) P−E loops between 23 and 400 °C collected with 10 kHz bipolar voltage waveform. (b) Temperature−dependent leakage current density (J) over bias between 23 and 400 °C. Comparison of (c) ∆Ec/2 and (d) Pr results from this work with Mizutani et al. [21], Zhu et al. [20], Gund et al. [22], and Wang et al. [20]. The results in (a,b) are from this work, while (c,d) are a comparison of our results with previous reports.
Micromachines 13 00887 g003
Figure 4. Polarization retention after poling in either (a) nitrogen or (b) metal surface state and dwelling up to 1000 s at the indicated temperature.
Figure 4. Polarization retention after poling in either (a) nitrogen or (b) metal surface state and dwelling up to 1000 s at the indicated temperature.
Micromachines 13 00887 g004
Figure 5. Ferroelectric fatigue exhibits a strong dependence on the measurement temperature. (a) Normalized Pr dependence on cycles for temperatures between 23 and 400 °C with error bars of a standard deviation. Representative P–E loops throughout the fatigue cycling for (b) 23 °C, (c) 100 °C, (d) 200 °C, (e) 300 °C, and (f) 400 °C. The colors of the plot borders for (bf) correspond to the temperature of the measurement in (a), and the different traces in (bf) are consistent for ease of comparison.
Figure 5. Ferroelectric fatigue exhibits a strong dependence on the measurement temperature. (a) Normalized Pr dependence on cycles for temperatures between 23 and 400 °C with error bars of a standard deviation. Representative P–E loops throughout the fatigue cycling for (b) 23 °C, (c) 100 °C, (d) 200 °C, (e) 300 °C, and (f) 400 °C. The colors of the plot borders for (bf) correspond to the temperature of the measurement in (a), and the different traces in (bf) are consistent for ease of comparison.
Micromachines 13 00887 g005
Publisher’s Note: MDPI stays neutral with regard to jurisdictional claims in published maps and institutional affiliations.

Share and Cite

MDPI and ACS Style

Drury, D.; Yazawa, K.; Zakutayev, A.; Hanrahan, B.; Brennecka, G. High-Temperature Ferroelectric Behavior of Al0.7Sc0.3N. Micromachines 2022, 13, 887. https://doi.org/10.3390/mi13060887

AMA Style

Drury D, Yazawa K, Zakutayev A, Hanrahan B, Brennecka G. High-Temperature Ferroelectric Behavior of Al0.7Sc0.3N. Micromachines. 2022; 13(6):887. https://doi.org/10.3390/mi13060887

Chicago/Turabian Style

Drury, Daniel, Keisuke Yazawa, Andriy Zakutayev, Brendan Hanrahan, and Geoff Brennecka. 2022. "High-Temperature Ferroelectric Behavior of Al0.7Sc0.3N" Micromachines 13, no. 6: 887. https://doi.org/10.3390/mi13060887

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.

Article Metrics

Back to TopTop