Next Article in Journal
Defect Detection and Depth Estimation in Composite Materials for Pulsed Thermography Images by Nonuniform Heating Correction and Oriented Gradient Information
Next Article in Special Issue
Properties of PBZTS Ferroelectric Ceramics Obtained Using Spark Plasma Sintering
Previous Article in Journal
Effectiveness of Self-Adhesive Resin Luting Cement in CAD-CAM Blocks—A Systematic Review and Meta-Analysis
Previous Article in Special Issue
Crystal Structure and Electrical Properties of Ruthenium-Substituted Calcium Copper Titanate
 
 
Font Type:
Arial Georgia Verdana
Font Size:
Aa Aa Aa
Line Spacing:
Column Width:
Background:
Communication

The Enhanced Thermal Stability of (Mg0.95Ni0.05)2TiO4 Dielectric Ceramics Modified by a Multi-Phase Method

1
Department of Electronic Engineering, Ming Chuan University, Taoyuan City 333, Taiwan
2
Department of Mechanical Engineering, National Taiwan University, Taipei 106, Taiwan
3
Department of Electronic Engineering and Organic Electronics Research Center, Ming Chi University of Technology, New Taipei City 243, Taiwan
*
Authors to whom correspondence should be addressed.
Materials 2023, 16(8), 2997; https://doi.org/10.3390/ma16082997
Submission received: 19 March 2023 / Revised: 1 April 2023 / Accepted: 6 April 2023 / Published: 10 April 2023
(This article belongs to the Special Issue Advances in Dielectric Ceramics)

Abstract

:
The thermal stability of (Mg0.95Ni0.05)2TiO4 dielectric ceramics has been improved by mixing with CaTiO3 phases owing to higher positive temperature coefficients. The pure (Mg0.95Ni0.05)2TiO4 and the mixture phase systems of CaTiO3-modified (Mg0.95Ni0.05)2TiO4 were verified by XRD diffraction patterns to ensure the crystallite of different phases. The microstructures of the CaTiO3-modified (Mg0.95Ni0.05)2TiO4 were observed by SEM and EDS to investigate the relation between element ratios and grains. As a result, it can be seen that the thermal stability of the CaTiO3-modified (Mg0.95Ni0.05)2TiO4 can be effectively enhanced, compared with the pure (Mg0.95Ni0.05)2TiO4. Moreover, the radio frequency dielectric performances of CaTiO3-modified (Mg0.95Ni0.05)2TiO4 dielectric ceramics are strongly dependent upon the density and the morphology of the specimens. The champion sample with the ratio of (Mg0.95Ni0.05)2TiO4 and CaTiO3 of 0.92:0.08 showed an εr value of 19.2, an Qf value of 108,200 GHz, and a τf value of −4.8 ppm/°C, which may encourage (Mg0.95Ni0.05)2TiO4 ceramics to broaden the range of novel applications and match the requirements of 5G or next-generation communication systems.

1. Introduction

As a result of the continuous evolution of science and technology, millimeter-wave technology has been extensively developed and considered as a branch of 5G communication or next-generation mobile communication technology. Due to a large amount of data transmission, a multilayer board is required as the main circuit board design, leading to materials which should possess both low dielectric loss and conductor loss characteristics [1,2,3,4,5]. Dielectric materials, to date, are a good choice for creating high-frequency components that have a higher dielectric constant (εr), which can contribute to the miniaturization of components; high-quality factors (Qf values) can improve the energy of stored electromagnetic waves and the temperature coefficient of the resonance frequency (τf) approaching zero, which can enhance the thermal stability of the components. For example, when a filter possesses the three abovementioned characteristics, the filter results in effective downsizing, lower dielectric loss rates, greater filtering activity, and greater stability, unaffected by the external ambient temperature [6,7].
The ceramic systems based on MgTiO3 have always received considerable attention and applications in the literature. For example, dielectric passive components of MgTiO3 in a communication system have been employed to be a resonator, duplex, filter, and antenna [8,9,10,11,12]. Therefore, it is considerably important to enhance the dielectric performance of MgTiO3. When the ratio of Mg and Ti is 2:1, the binary titanate ceramic Mg2TiO4 possesses a spinel-type structure that belongs to the cubic phase with Fd-3m space group (2 2 7). It demonstrates an εr value of 14, a Qf value of 150,000 GHz, and a τf value of −50 ppm/°C [13,14,15]. In addition, to further improve the dielectric characteristics, the method of partial substitution that selects Ni2+ (0.069 nm) with a radius resembling Mg2+ (0.078 nm) to perform the substitution was presented [16]. When the Mg2+ ions were replaced by Ni2+ ions to form (Mg, Ni)2TiO4 compositions, the (Mg0.95Ni0.05)2TiO4 compositions possessing a spinel-type structure presented a good dielectric performance with an εr value of 16.43, a Qf value of 238,000 GHz, and a τf value of −55 ppm/°C [17]. Moreover, an inferior (Mg0.95Ni0.05)TiO3 phase also appeared during the synthesizing of (Mg0.95Ni0.05)2TiO4, which may be attributed to the effect of the thermal decomposition mechanism [18]. However, the slight (Mg0.95Ni0.05)TiO3-doped (Mg0.95Ni0.05)2TiO4 possess a comparable performance, with an εr value of 17.2, a Qf value of 180,000 GHz, and a τf value of −45 ppm/°C [19], compared to those of the pure (Mg0.95Ni0.05)2TiO4 composition [17].
On the other hand, a multi-phase method has been employed to modify the dielectric characteristics. In Mg2TiO4–SrTiO3 systems [20], Mg2TiO4 and SrTiO3 have spinal cubic (lattice parameters: a = 8.439 Å, space group Fd3m) (ICDD-PDF#00-003-0858) and cubic perovskite (ICDD-PDF#01-084-0443), respectively. When x increased, the peak intensity of SrTiO3 increased and the lattice parameters of Mg2TiO4 remained unchanged, which demonstrates that the two-phase system was used to modify relative permittivity in the Mg2TiO4–SrTiO3 system. In (Mg0.95Zn0.05)2TiO4–SrTiO3 systems [21], the lattice parameters had slight influence and remained unchanged after the SrTiO3 was added into (Mg0.95Zn0.05)2TiO4, which confirms that the presence of a two-phase system could effectively promote densification in the (Mg0.95Zn0.05)2TiO4 matrix. In addition, CaTiO3- and SrTiO3-modified (Mg0.95Co0.05)2TiO4 ceramics [22,23] were presented using a multi-phase method for low–loss dielectric properties at microwave frequencies. Furthermore, thermal stability of dielectric ceramics is another important factor in practical applications. However, few studies have been conducted to discuss the thermal stability of (Mg0.95Ni0.05)2TiO4. For this purpose, we have made great efforts to enhance the thermal stability factor of (Mg0.95Ni0.05)2TiO4 compositions using a perovskite structured SrTiO3 additive to form a two-phase system in our previous report [24].
In this study, we demonstrate the microstructure and radio frequency dielectric characteristics of the CaTiO3-modified (Mg0.95Ni0.05)2TiO4 ceramic system for enhancing its thermal stability factor using the multi-phase method. We attempted to add CaTiO3 with a high positive temperature coefficient to form a three-phase system and to compensate the negative temperature coefficient of (Mg0.95Ni0.05)2TiO4. X-ray diffraction (XRD), scanning electron microscopy (SEM), and energy-dispersive X-ray spectrometer (EDS) analyses were also employed to study the microstructure grain boundary, and compositions of the ceramic system. The radio frequency dielectric performances of the CaTiO3-modified (Mg0.95Ni0.05)2TiO4 were quantified and examined by employing the formation of muti-phase coexistence.

2. Materials and Method

In this study, (Mg0.95Ni0.05)2TiO4 and CaTiO3 were produced by a mixed-oxide solid-state reaction using the following high-purity chemical powders: magnesium oxide (MgO), nickel oxide (NiO), calcium carbonate (CaCO3), and titanium dioxide (TiO2). Because MgO is hygroscopic in nature, it first removes the moisture remaining at 600 °C for 2 h. The mixture of the above oxides was mixed according to the stoichiometries of (Mg0.95Ni0.05)2TiO4 and CaTiO3. They were then ball ground in distilled water (ball grinding medium) for 24 h. All mixed powders were parched in a kiln and pre-phased (calcine) at 1100 °C for 4 h in a high-temperature furnace. Then, the pre-phased reagents were mixed again according to the chemical molar ratio of (1–x) (Mg0.95Ni0.05)2TiO4∙xCaTiO3, and ball ground into a fine powder for 24 h. Then, polyvinyl alcohol (PVA 500; Showa, Tokyo, Japan) as a binder was added to the calcined powder, uniformly granulated, screened with a 100-mesh screen, and compressed with a pressure of 200 MPa to form a tablet form with a height of 0.5 cm and diameter of 1.1 cm. The sintering temperatures of the tablets were set at 1300~1425 °C for 4 h in air. The risen and dropped temperature rates were set at 10 °C/min for all samples.
The crystallization-phase observation of the pre-phased powder and mixture compositions were analyzed by XRD (Rigaku D/Max III. V., Tx for USA) The lattice constant was calculated using the Rietveld method to fit the XRD patterns. SEM (Philips XL-40FEG, Eindhoven, The Netherlands) was employed to observe the surface morphologies of samples, and EDS was utilized to demonstrate the different phases and compositions. The apparent densities of the samples were measured using the Archimedes method. The εr and Qf values at radio frequencies were measured by the Hakki–Coleman dielectric resonator method [25,26,27].
The measurement was mainly composed of a vector network analyzer (HP8757D, Agilent Technologies, Taipei, Taiwan) and sweep oscillator connections (HP8350B, Agilent Technologies, Taipei, Taiwan). The thermal stability ( τ f values) was evaluated with a temperature range from 20 to 80 °C. The following Formula (1) was utilized to obtain the τf value (ppm/°C):
τ f = f 2 f 1 f 1 T 2 T 1    
where f1 and f2 represent the resonant frequencies at T1 and T2, respectively.

3. Results and Discussion

Figure 1 presents the XRD patterns of the (1–x) (Mg0.95Ni0.05)2TiO4∙xCaTiO3 with an x value of 0.08 after sintering at different temperatures for 4 h. According to the JCPDS card, a three-phase system can be observed, which consisted of (Mg0.95Ni0.05)2TiO4 phase with a spinel-type structure as the primary crystalline phase (Mg2TiO4, ICDD–PDF#00-025-1157; lattice constants a = b = c = 0.84409 nm), (Mg0.95Ni0.05)TiO3 phase (MgTiO3, ICDD–PDF#00-006-0494), and a CaTiO3 phase with perovskite structure (JCPDS #22-0153). The lattice constant was slightly decreased with the increasing sintering temperature (a = b = c from 0.84005 to 0.83456 nm), indicating sharper main peaks of the (Mg0.95Ni0.05)2TiO4 phase and larger grain size. No other obvious phases and impurities were identified in Figure 1. In addition, the reason for the presence of the (Mg0.95Ni0.05)TiO3 phase is generally considered to be the uneven particle size of the initial materials, which increases the probability of secondary crystallization nucleation. Another reason for the formation of the (Mg0.95Ni0.05)TiO3 phase may be the effect of the thermal decomposition mechanism [18]. However, the ratio of (Mg0.95Ni0.05)TiO3 phase in the ceramics was decreased due to the increased grain boundary motion with the increasing sintering temperature, as shown in Table 1. Moreover, the (Mg0.95Ni0.05)TiO3 had no noticeable impact on the dielectric properties of (Mg0.95Ni0.05)2TiO4 in our previous study [19]. Therefore, the influence of the inferior (Mg0.95Ni0.05)TiO3 phase can be negligible when the sintering temperature is over 1350 °C.
Figure 2 presents the results of the XRD analysis of the (1–x) (Mg0.95Ni0.05)2TiO4 xCaTiO3 with different x values. It can be observed that the different contents have no obvious influence on the phase growth of the (Mg0.95Ni0.05)2TiO4. A few (Mg0.95Ni0.05)TiO3 peaks still existed in all patterns. As mentioned above, the effect of the inferior (Mg0.95Ni0.05)TiO3 phase on dielectric performance is quite slight and can be neglected. The lattice constant of the (Mg0.95Ni0.05)2TiO4 with a different amount of the CaTiO3 contents is presented in Table 2. It was also observed that all samples have a spinal cubic structure with the lattice constants (a = b = c) from 0.84005 to 0.83456 nm, indicating that the (Mg0.95Ni0.05)2TiO4 is still in the primary phase. When CaTiO3 was blended with (Mg0.95Ni0.05)2TiO4, no obvious influence on the lattice constants of (Mg0.95Ni0.05)2TiO4 could be found (Table 2). Furthermore, the growth of mixed phases in the one ceramic may cause a negative effect due to structural dissimilarities and the larger ionic radii values of Ca2+ (0.106 nm) compared to those of Mg2+ (0.078 nm) and Ni2+ (radii = 0.069 nm) [16]. However, the XRD analysis confirms the coexistence of the multiple phases without the structural dissimilarities in our samples.
Figure 3 shows the SEM images of the morphologies of the 0.92∙(Mg0.95Ni0.05)2TiO4∙0.08CaTiO3 sintered at different temperatures. When the sintering temperature was increased, the grain size increased in Figure 3a–f, which is consistent with the XRD results (Figure 1). The pores reduced with the sintering temperature increasing from 1300 to 1350 °C. The reason for the increase in the grain size and the decrease in pores is the thermal drive energy, which enables connection and expands the neck between the grains. Therefore, Figure 3a–c exhibits the grain growth with better movement of the grain boundary and a more uniform and dense morphology. However, when the sintering temperature was increased from 1350 to 1425 °C, the grain size still increased, and the pore size became larger. This is attributed to the excessive extrusion between grains and air pressure under too-high sintering temperatures, which is similar with previous reports [20,21,22,23,24]. Furthermore, grains of 0.92∙(Mg0.95Ni0.05)2TiO4∙0.08CaTiO3 can be roughly divided into three shapes, as shown in Figure 3c. The EDS results of each grain are summarized in Table 3. Therefore, the different grains were identified as follows: spot A is (Mg0.95Ni0.05)TiO3; spot B is (Mg0.95Ni0.05)2TiO4’ and spot C is CaTiO3. The EDS results are consistent with the XRD analysis, verifying that the (1–x) (Mg0.95Ni0.05)2TiO4∙xCaTiO3 is a three-phase coexistence system.
Figure 4 shows the results of the apparent density and dielectric constant (εr values) of the (1–x) (Mg0.95Ni0.05)2TiO4∙xCaTiO3 with different x values and temperatures. The apparent density was increased with the increasing x value because CaTiO3 (~4.036 g/cm3) possesses a higher density than that of (Mg0.95Ni0.05)2TiO4 (~3.49 g/cm3) [17]. Moreover, the apparent density value increased when the temperature increased from 1300 to 1350 °C, which is due to the grain growth (Figure 3a–c). However, the apparent density was reduced due to the enlarged pore size (Figure 3d–f) when the temperature increased from 1350 to 1425 °C. These results lead to the optimal sintering temperature of 1350 °C being obtained. Due to much higher dielectric constant (εr) of (Mg0.95Ni0.05)2TiO4 (~16.4) and CaTiO3 (~170) than that of air (~1), the εr of the (1–x) (Mg0.95Ni0.05)2TiO4 xCaTiO3 correlates positively with apparent density. Therefore, the εr changed with the change in the apparent density and the x value. Therefore, the dielectric constant changes from 18.6 to 20.9 as x increases from 0.06 to 0.12, as shown in Table 4.
Figure 5 shows that the Qf value (quality factor) of the (1–x) (Mg0.95Ni0.05)2TiO4 xCaTiO3 decreased with the increasing the x value. It is attributed to the fact that the Qf value of CaTiO3 (~3600 GHz) was relatively smaller than that of (Mg0.95Ni0.05)2TiO4 (~238,000 GHz). In addition, the Qf of the (1–x) (Mg0.95Ni0.05)2TiO4∙xCaTiO3 rises at 1300–1350 °C and drops at 1350–1425 °C in Figure 5. Compared with Figure 4, the Qf of the (1–x) (Mg0.95Ni0.05)2TiO4 xCaTiO3 correlated positively with the εr and apparent density. Although there are many factors that impact the Qf, such as dielectric loss (which is caused by the second phase), oxygen vacancy, grain size, and porosity [28], the Qf is mainly dependent on the apparent density in our case. Similar with the results of the apparent density at different temperatures (Figure 4), the Qf also reached the optimal value at 1350 °C, as listed in Table 4. The τf of the (1–x) (Mg0.95Ni0.05)2TiO4∙xCaTiO3 sintered at different temperatures seems to maintain a constant value, which is strongly dependent on the CaTiO3 contents (x value), as shown in Figure 5 and Table 4. The composition and phase determined the thermal stability of the (1–x) (Mg0.95Ni0.05)2TiO4∙xCaTiO3 because a high positive temperature coefficient of CaTiO3 can compensate the negative temperature coefficient of (Mg0.95Ni0.05)2TiO4. Therefore, the τf was changed from −20.7 to 30.5 (ppm/°C) when x increased from 0.04 to 0.12, indicating that τf = 0 is possible after controlling x. It is worth noting that the τf was only −4.8 ppm/°C at x = 0.08 but the Qf was kept at 108,200 GHz.

4. Conclusions

In conclusion, the thermal stability of the CaTiO3-modified (Mg0.95Ni0.05)2TiO4 ceramic system was investigated. The dense morphology without pores can be obtained at 1350 °C, resulting in the optimal sintering temperature of the apparent density, εr, and Qf. A high positive temperature coefficient of CaTiO3 can be used to improve the thermal stability of (Mg0.95Ni0.05)2TiO4. The τf can be adjusted with changing the CaTiO3 contents, even closing to zero. The excellent dielectric characteristics of the 0.92∙(Mg0.95Ni0.05)2TiO4∙0.08CaTiO3 sintered at 1350 °C was presented with an εr of 19.2, an Qf of 108,200 GHz, and a τf of −4.8 ppm/°C. Therefore, the CaTiO3-modified (Mg0.95Ni0.05)2TiO4 ceramic system showed high thermal stability and performance, suggesting the potential of these ceramics as dielectric substrate materials and radio frequency passive components in the microwave field to miniaturize components and transmit signals neglecting the temperature factor.

Author Contributions

C.-H.S. wrote the manuscript and performed the experiment; T.-Y.H., K.-C.L., S.-H.H., C.-H.W. and Y.-T.L. performed the experiment; Z.-L.T. contributed to the analysis the results; Z.-L.T. financially supported the research materials and publication fees; C.-H.S., T.-W.S., W.-F.W. and Z.-L.T. revised the manuscript. All authors have read and agreed to the published version of the manuscript.

Funding

This research received no external funding.

Conflicts of Interest

The authors declare no conflict of interest.

References

  1. Freitas, A.E.; Manhabosco, T.M.; Batista, R.J.C.; Segundo, A.K.R.; Araújo, H.X.; Araújo, F.G.S.; Costa, A.R. Development and Characterization of Titanium Dioxide Ceramic Substrates with High Dielectric Permittivities. Materials 2020, 13, 386. [Google Scholar] [CrossRef] [PubMed]
  2. Aljaafari, A.; Sedky, A. Influence of Fine Crystal Percentage on the Electrical Properties of ZnO Ceramic-Based Varistors. Crystals 2020, 10, 681. [Google Scholar] [CrossRef]
  3. Yu, H.; Luo, T.; He, L.; Liu, J. Effect of ZnO on Mg2TiO4–MgTiO3–CaTiO3 Microwave Dielectric Ceramics Prepared by Reaction Sintering Route. Adv. Appl. Ceram. 2019, 118, 98–105. [Google Scholar] [CrossRef]
  4. Zhai, S.; Liu, P.; Fu, Z. Microwave Dielectric Properties of Low-Fired [Mg0.98(Li0.5Bi0.5)0.02]2SiO4–Ca0.8Sm0.4/3TiO3 Composite Ceramics. J. Mater. Sci. Mater. Electron. 2018, 29, 1298–1303. [Google Scholar] [CrossRef]
  5. Palmero, P. Structural Ceramic Nanocomposites: A Review of Properties and Powders’ Synthesis Methods. Nanomaterials 2015, 5, 656–696. [Google Scholar] [CrossRef]
  6. Tang, B.; Xiang, Q.; Fang, Z.; Zhang, X.; Xiong, Z.; Li, H.; Yuan, C.; Zhang, S. Influence of Cr3+ Substitution for Mg2+ on the Crystal Structure and Microwave Dielectric Properties of CaMg1-XCr2x/3Si2O6 Ceramics. Ceram. Int. 2019, 45, 11484–11490. [Google Scholar] [CrossRef]
  7. Yuan, S.; Gan, L.; Ning, F.; An, S.; Jiang, J.; Zhang, T. High-Q×f 0.95 MgTiO3–0.05CaTiO3 Microwave Dielectric Ceramics with the Addition of LiF Sintered at Medium Temperatures. Ceram. Int. 2018, 44, 20566–20569. [Google Scholar] [CrossRef]
  8. Gogoi, P.; Singh, L.R.; Pamu, D. Characterization of Zn Doped MgTiO3 Ceramics: An Approach for RF Capacitor Applications. J. Mater. Sci. Mater. Electron. 2017, 28, 11712–11721. [Google Scholar] [CrossRef]
  9. Ullah, A.; Iqbal, Y.; Mahmood, T.; Mahmood, A.; Naeem, A.; Hamayun, M. Kinetic Analysis on the Synthesis of Mg0.95Zn0.05TiO3 Microwave Dielectric Ceramic by Polymeric Precursor Method. Ceram. Int. 2015, 41, 15089–15096. [Google Scholar] [CrossRef]
  10. Huang, C.L.; Pan, C.L.; Hsu, J.F. Dielectric Properties of (1−x)(Mg0.95Co0.05)TiO3–xCaTiO3 Ceramic System at Microwave Frequency. Mater. Res. Bull. 2002, 37, 2483–2490. [Google Scholar] [CrossRef]
  11. Sohn, J.H.; Inaguma, Y.; Yoon, S.O.; Itoh, M.; Nakamura, T.; Yoon, S.J.; Kim, H.J. Microwave Dielectric Characteristics of Ilmenite-Type Titanates with High Q Values. Jpn. J. Appl. Phys. 1994, 33, 5466. [Google Scholar] [CrossRef]
  12. Wakino, K. Recent Development of Dielectric Resonator Materials and Filters in Japan. Ferroelectrics 1989, 91, 69–86. [Google Scholar] [CrossRef]
  13. Isobe, M.; Ueda, Y. Synthesis, Structure and Physical Properties of Spinel Solid Solutions Mg2TiO4–MgTi2O4. J. Alloy. Compd. 2004, 383, 85–88. [Google Scholar] [CrossRef]
  14. Belous, A.; Ovchar, O.; Durilin, D.; Krzmanc, M.M.; Valant, M.; Suvorov, D. High-Q Microwave Dielectric Materials Based on the Spinel Mg2TiO4. J. Am. Ceram. Soc. 2006, 89, 3441–3445. [Google Scholar] [CrossRef]
  15. Belous, A.; Ovchar, O.; Durylin, D.; Valant, M.; Macek-Krzmanc, M.; Suvorov, D. Microwave Composite Dielectrics Based on Magnesium Titanates. J. Eur. Ceram. Soc. 2007, 27, 2963–2966. [Google Scholar] [CrossRef]
  16. Shannon, R.D. Revised Effective Ionic Radii and Systematic Studies of Interatomic Distances in Halides and Chalcogenides. Acta Cryst. A 1976, 32, 751–767. [Google Scholar] [CrossRef]
  17. Huang, C.L.; Ho, C.E. Microwave Dielectric Properties of (Mg1−xNix)2TiO4 (x=0.02–0.1) Ceramics. Int. J. Appl. Ceram. Technol. 2010, 7, E163–E169. [Google Scholar] [CrossRef]
  18. Petrova, M.A.; Mikirticheva, G.A.; Novikova, A.S.; Popova, V.F. Spinel Solid Solutions in the Systems MgAl2O4–ZnAl2O4 and MgAl2O4–Mg2TiO4. J. Mater. Res. 1997, 12, 2584–2588. [Google Scholar] [CrossRef]
  19. Shen, C.H.; Pan, C.L.; Lin, S.H. A Study of the Effect of Sintering Conditions of Mg0. 95Ni0. 05Ti3 on Its Physical and Dielectric Properties. Molecules 2020, 25, 5988. [Google Scholar] [CrossRef]
  20. Huang, C.L.; Liu, S.S. Dielectric Characteristics of the (1−x)Mg2TiO4–xSrTiO3 Ceramic System at Microwave Frequencies. J. Alloy. Compd. 2009, 471, L9–L12. [Google Scholar] [CrossRef]
  21. Huang, C.L.; Wang, J.J.; Chang, Y.P. Dielectric Properties of Low Loss (1–x)(Mg0.95Zn0.05)TiO3–xSrTiO3 Ceramic System at Microwave Frequency. J. Am. Ceram. Soc. 2007, 90, 858–862. [Google Scholar] [CrossRef]
  22. Huang, C.L.; Liu, S.S.; Chen, S.H. Dielectric Properties of a New Ceramic System (Mg0.95Zn0.05)2TiO4–CaTiO3 at Microwave Frequencies. Jpn. J. Appl. Phys. 2009, 48, 071402. [Google Scholar] [CrossRef]
  23. Huang, C.L.; Chen, J.Y. Low-Loss Microwave Dielectrics Using SrTiO3-Modified (Mg0.95Co0.05)2TiO4 Ceramics. J. Alloy. Compd. 2009, 485, 706–710. [Google Scholar] [CrossRef]
  24. Shen, C.H.; Pan, C.L. Dielectric Properties and Applications of Low-Loss (1−x)(Mg0.95Ni0.05)2TiO4-xSrTiO3 Ceramic System at Microwave Frequency. Int. J. Appl. Ceram. Technol. 2015, 12, E127–E133. [Google Scholar] [CrossRef]
  25. Kobayashi, Y.; Katoh, M. Microwave Measurement of Dielectric Properties of Low-Loss Materials by the Dielectric Rod Resonator Method. IEEE Trans. Microw. Theory Tech. 1985, 33, 586–592. [Google Scholar] [CrossRef]
  26. Courtney, W.E. Analysis and Evaluation of a Method of Measuring the Complex Permittivity and Permeability Microwave Insulators. IEEE Trans. Microw. Theory Tech. 1970, 18, 476–485. [Google Scholar] [CrossRef]
  27. Hakki, B.W.; Coleman, P.D. A Dielectric Resonator Method of Measuring Inductive Capacities in the Millimeter Range. IRE Trans. Microw. Theory Tech. 1960, 8, 402–410. [Google Scholar] [CrossRef]
  28. Silverman, B.D. Microwave Absorption in Cubic Strontium Titanate. Phys. Rev. 1962, 125, 1921–1930. [Google Scholar] [CrossRef]
Figure 1. X-ray diffraction patterns of 0.92∙(Mg0.95Ni0.05)2TiO4∙0.08CaTiO3 sintered at different temperatures for 4 h.
Figure 1. X-ray diffraction patterns of 0.92∙(Mg0.95Ni0.05)2TiO4∙0.08CaTiO3 sintered at different temperatures for 4 h.
Materials 16 02997 g001
Figure 2. X-ray diffraction patterns of (1–x) (Mg0.95Ni0.05)2TiO4∙xCaTiO3 sintered at 1350 °C for 4 h.
Figure 2. X-ray diffraction patterns of (1–x) (Mg0.95Ni0.05)2TiO4∙xCaTiO3 sintered at 1350 °C for 4 h.
Materials 16 02997 g002
Figure 3. SEM images of 0.92∙(Mg0.95Ni0.05)2TiO4∙0.08CaTiO3 sintered at (a) 1300, (b) 1325, (c) 1350, (d) 1375, (e) 1400, and (f) 1425 °C for 4 h.
Figure 3. SEM images of 0.92∙(Mg0.95Ni0.05)2TiO4∙0.08CaTiO3 sintered at (a) 1300, (b) 1325, (c) 1350, (d) 1375, (e) 1400, and (f) 1425 °C for 4 h.
Materials 16 02997 g003
Figure 4. The apparent density and dielectric constant (εr values) of the (1–x) (Mg0.95Ni0.05)2TiO4∙xCaTiO3 sintered at different temperatures.
Figure 4. The apparent density and dielectric constant (εr values) of the (1–x) (Mg0.95Ni0.05)2TiO4∙xCaTiO3 sintered at different temperatures.
Materials 16 02997 g004
Figure 5. Qf and τf values of the (1−x) (Mg0.95Ni0.05)2TiO4∙xCaTiO3 sintered at different temperatures for 4 h.
Figure 5. Qf and τf values of the (1−x) (Mg0.95Ni0.05)2TiO4∙xCaTiO3 sintered at different temperatures for 4 h.
Materials 16 02997 g005
Table 1. The lattice parameter and compositions of 0.92∙(Mg0.95Ni0.05)2TiO4 0.08CaTiO3 sintered at different temperatures for 4 h. (Mg0.95Ni0.05)TiO3 and CaTiO3 ratios are determined by all peak areas of each phase.
Table 1. The lattice parameter and compositions of 0.92∙(Mg0.95Ni0.05)2TiO4 0.08CaTiO3 sintered at different temperatures for 4 h. (Mg0.95Ni0.05)TiO3 and CaTiO3 ratios are determined by all peak areas of each phase.
Temperaturesa = b = c (nm)(Mg0.95Ni0.05)TiO3 Ratio (%)CaTiO3 Ratio (%)
13000.84005 ± 0.103317.411.6
13250.84005 ± 0.103317.213.4
13500.83986 ± 0.09721713.5
13750.83456 ± 0.099514.913.8
14000.83456 ± 0.099514.713.8
14250.83456 ± 0.099514.414.1
Table 2. The lattice parameter and compositions of (1–x) (Mg0.95Ni0.05)2TiO4∙xCaTiO3 sintered at 1350 °C for 4 h. (Mg0.95Ni0.05)TiO3 and CaTiO3 ratios are determined by all peak areas of each phase.
Table 2. The lattice parameter and compositions of (1–x) (Mg0.95Ni0.05)2TiO4∙xCaTiO3 sintered at 1350 °C for 4 h. (Mg0.95Ni0.05)TiO3 and CaTiO3 ratios are determined by all peak areas of each phase.
x Valuesa = b = c (nm)(Mg0.95Ni0.05)TiO4 Ratio (%)CaTiO3 Ratio (%)
0.060.84005 ± 0.103317.19.6
0.080.84005 ± 0.10331713.5
0.090.83986 ± 0.097214.513.5
0.10.83456 ± 0.099513.313.7
0.120.83456 ± 0.09951414.4
Table 3. Composition analysis from EDS results for spot A, B, and C in Figure 3c.
Table 3. Composition analysis from EDS results for spot A, B, and C in Figure 3c.
Atom (%)
SpotMgNiCaTiO
A17.542.2016.8463.42
B24.272.25019.5153.97
C0020.4219.4960.09
Table 4. Microwave dielectric performances of (1–x) (Mg0.95Ni0.05)2TiO4 xCaTiO3 at 1350 °C for 4 h.
Table 4. Microwave dielectric performances of (1–x) (Mg0.95Ni0.05)2TiO4 xCaTiO3 at 1350 °C for 4 h.
x ValuesDensity
(g/cm3)
εr ValuesQf Values (GHz)τf Values
(ppm/°C)
0.063.4418.6131,000−20.7
0.083.4819.2108,200−4.8
0.093.5119.690,0001.3
0.13.5320.175,00013.9
0.123.5620.958,00030.5
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content.

Share and Cite

MDPI and ACS Style

Shen, C.-H.; Shen, T.-W.; Hsieh, T.-Y.; Lan, K.-C.; Hsu, S.-H.; Wang, C.-H.; Lin, Y.-T.; Wu, W.-F.; Tseng, Z.-L. The Enhanced Thermal Stability of (Mg0.95Ni0.05)2TiO4 Dielectric Ceramics Modified by a Multi-Phase Method. Materials 2023, 16, 2997. https://doi.org/10.3390/ma16082997

AMA Style

Shen C-H, Shen T-W, Hsieh T-Y, Lan K-C, Hsu S-H, Wang C-H, Lin Y-T, Wu W-F, Tseng Z-L. The Enhanced Thermal Stability of (Mg0.95Ni0.05)2TiO4 Dielectric Ceramics Modified by a Multi-Phase Method. Materials. 2023; 16(8):2997. https://doi.org/10.3390/ma16082997

Chicago/Turabian Style

Shen, Chun-Hsu, Ting-Wei Shen, Tsai-Yu Hsieh, Kai-Chun Lan, Shen-Hsien Hsu, Ching-Hsuan Wang, Yu-Ting Lin, Wen-Fang Wu, and Zong-Liang Tseng. 2023. "The Enhanced Thermal Stability of (Mg0.95Ni0.05)2TiO4 Dielectric Ceramics Modified by a Multi-Phase Method" Materials 16, no. 8: 2997. https://doi.org/10.3390/ma16082997

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.