Next Article in Journal
Sustainable Use of Sludge from Industrial Park Wastewater Treatment Plants in Manufacturing Lightweight Aggregates
Next Article in Special Issue
Improved Anti-Vulcanization and Bonding Performance of a Silver Alloy Bonding Wire by a Cathodic Passivation Treatment with Palladium
Previous Article in Journal
Analysis of Engineering Characteristics and Microscopic Mechanism of Red Mud–Bauxite Tailings Mud Foam Light Soil
Previous Article in Special Issue
Designing High Entropy Bulk Metallic Glass (HE-BMG) by Similar Element Substitution/Addition
 
 
Font Type:
Arial Georgia Verdana
Font Size:
Aa Aa Aa
Line Spacing:
Column Width:
Background:
Article

Metallization on Sapphire and Low-Temperature Joining with Metal Substrates

1
School of Materials Science and Engineering, Wuhan University of Technology, Wuhan 430070, China
2
The Institute of Technological Science, Wuhan University, Wuhan 430072, China
*
Author to whom correspondence should be addressed.
Materials 2022, 15(5), 1783; https://doi.org/10.3390/ma15051783
Submission received: 31 December 2021 / Revised: 21 January 2022 / Accepted: 25 January 2022 / Published: 26 February 2022
(This article belongs to the Special Issue Physical Metallurgy of Metals and Alloys)

Abstract

:
To meet the packaging requirements of sapphire in special electronic components, there is an urgent need for a joining process that can realize a good connection between sapphire and dissimilar metals at a low temperature. In this work, the surface of a sapphire substrate was successfully catalytically activated and metallized by an electroless nickel plating process. Moreover, the solderability and interconnection of metallized sapphire with Sn-based solders were evaluated and investigated at 250 °C, and the wetting angle of the Sn-based solders on sapphire on sapphire without and with metallization was 125° and 51°, respectively. The interfacial microscopic morphology and element distribution in the Cu/Sn-Ag solder/sapphire solder joints were analyzed. It was found that the middle solder layer has diffused during the reflow process, inferring good adhesion between sapphire and Cu substrate with the aid of the Ni-P deposition. Thus, a sapphire welding method with a simple process suitable for practical applications is demonstrated.

1. Introduction

Sapphire has superior optical and mechanical properties, including high melting point, high hardness, strong corrosion resistance and good thermal conductivity, which makes sapphire highly demanded in electronics and scientific instruments [1,2]. For electronics, sapphire is required to achieve joining with common metals by a simple reflow process. Unfortunately, sapphire is hard to achieve reliable solder joints during the reflow process as it is an Al2O3 single crystal. Currently, enormous works have been conducted on sapphire welding by various processes. Metallization on the sapphire surface is an important method. Related research on metallization methods of sapphire is listed in Table 1. Another method is using solders with active additions of Ti, Al and Mg. For instance, Ti addition in solders can significantly promote the solder wettability on sapphire. Mu et al. systematically studied the wetting behaviors of a Sn-Ti alloy on sapphire by the solid drop method [3]. However, Ti-based solders were required to be brazed in a high-temperature vacuum environment, which has been reported by Ning et al. [4]. With the assistance of ultrasonic, the brazing temperature of sapphire solder joints can be greatly reduced. Cui et al. used an Al-4.5Cu-1.5Mg alloy as a filling metal to connect sapphire through ultrasonic-assisted hot dipping [5]. A dense transient layer formed at the metal–sapphire interface to achieve solid connections between sapphire and the aluminum alloy. At present, various related researches on sapphire welding have been conducted in the above aspects. Unfortunately, they all have shortcomings for electronics applications, including high joining temperature, specific active solder, auxiliary ultrasonic brazing and so on.
Electroless nickel plating is a conventional surface treatment technology for wide applications prospects [10,11,12,13,14], which has the advantages of uniform deposition, dense plating, good conductivity and good solderability [15,16]. Electroless nickel plating on porous alumina ceramics was achieved by Zhang et al. [17]. Dehchar et al. successfully deposited copper films on non-conductive epoxy glass substrates by electroless plating as well [18]. Currently, many works related to electroless nickel plating have been carried out on different ceramic substrates. However, the related research on electroless nickel plating on sapphire substrates has not been reported yet.
In this work, we realized the metallization on sapphire by electroless nickel plating and elaborated its deposition mechanism. Therefore, the Cu/solder/sapphire sandwich solder joints can be fabricated, and then the interfacial morphology of these solder joints can be observed. Moreover, the fracture mechanism of solder joints was also studied. Finally, sapphire substrates can be joined by a simple reflow process at a low temperature and low pressure.

2. Experimental Works

In this work, sapphire substrates (10 mm × 10 mm × 1 mm, α-Al2O3 single crystal, purity >99.9%) were used for electroless plating. To achieve electroless nickel plating on the sapphire surface, the influence of substrate pretreatment on sapphire was studied to successfully deposit electroless nickel plating. The surface roughness of the sapphire substrates was measured by an atomic force microscope (AFM, Nanoscope IV, Veeco, Suzhou, China). Different types of chemical etching solutions were chosen to prepare the smooth deposition of the coatings. After grinding, etching, sensitizing, activating and initial plating (25 s) of the sapphire substrates, the surface morphology of sapphire after each process was observed through a scanning electron microscope (SEM, MIRA 3, TESCAN, Shanghai, China). Moreover, the changes in the surface morphology of the substrates were compared and analyzed.
The electroless plating solution is an acidic solution composed of deionized water, nickel sulfate, sodium hypophosphite, sodium citrate and ammonium sulfate. Table 2 lists the chemical reagents and the corresponding electroless plating conditions. The crystal structure of Ni-P coating was also analyzed by X-ray diffraction (XRD, Smart SE, Rigaku, Tokyo, Japan). Afterwards, the surface morphology and chemical composition of the electroless deposition by SEM and EDS (MIRA 3, TESCAN, Shanghai, China), respectively.
A contact angle measuring instrument (JC2000D2, Shanghai zhongchen digital technic apparatus Co. Ltd, Shanghai, China) was used to test the wetting angle of the Sn-3Ag solder balls (diameter 760 μm, 1.6 mg weight/ball, Langfang Bangzhuang Electronic Materials Co. Ltd, Langfang, China) on the sapphire with and without metallization in an atmospheric environment at 240 °C. Afterwards, sandwich-structured Cu/solder/sapphire solder joints were prepared by the reflow process. Pure copper substrates (purity 99%, 5 mm × 5 mm × 1 mm) and nickel-plated sapphire substrates were used as the upper and lower substrates, while solder pastes were evenly plated on the sapphire surface by a 100 μm thick stainless mask to connect the substrates. Then, the assembled Cu/solder/sapphire sandwich structure was prepared in a crucible furnace (vacuum degree <10−3 Pa) at a peak reflow temperature of 250 °C for 60 min under a pressure of 0.2 Mpa. The macroscopic appearance of sapphire solder joints is shown in Figure 1. The interfacial microstructure, morphology and element distribution of the sapphire solder joints and shear fracture surface were observed by SEM and EDS.

3. Results and Discussion

3.1. Metallization Mechanism on Sapphire

The surface activity of sapphire is rather poor and cannot auto catalyze, so the pretreatment is very important for deposition on the sapphire surface. The pretreatment process mainly includes surface degreasing, polishing, chemical etching, chemical sensitization and activation. The roughness of the polished and smooth surface measured by atomic force microscope (AFM) was 84.0 nm and 1.79 nm, respectively. Some works show that substrates with reasonable surface roughness can provide good anchorage for Ni-P films, which can significantly improve deposition adhesion [19,20]. After grinding, the deposition area between the coating and sapphire is greatly increased, thereby improving the bonding force of the deposit. Chemical treatment is also carried out to further improve the bonding force. Since the substrate is α-Al2O3, which is the most stable phase in the majority of alumina and is generally insoluble in acids and alkalis. In the subsequent electroless plating process, a mixed solution of HF and HCl was used as the coarsening solution. Therefore, Ni-P coating can be deposited on the sapphire, indicating that the coarsening solution can react with α-Al2O3 and form enormous micro-holes on the substrates. Thus, the substrate can be activated for the following electroless plating. During the plating process, a complete Ni-P coating can be directly deposited on the sapphire surface at once. The results show that sapphire can be metallized by a simple electroless plating process with proper pretreatments.
Figure 2 shows the surface morphology of sapphire substrates in each pretreatment process. Figure 2a–d is the substrate surface after grinding, etching, activating and initial plating, respectively. Figure 2a,b has a similar microstructure, while the surface morphology in Figure 2b is smoother. This is contributed to the etching solution that can react with the sapphire substrates. Figure 2c shows the morphology of sapphire substrates after activation by SnCl2/HCl and PdCl2/HCl solution. When the specimens absorbed with Sn+2 ions were immersed in the dilute PdCl2 solution, the Pd+2 ion was reduced to Pd metal and acted as a catalyst to initiate the deposition reaction according to Equation (1). As a result, some individual Pd patches can be formed on the sapphire surface, as shown in Figure 3.
S n + 2 + P d + 2 S n + 4 + P d  
Figure 2d exhibits the surface morphology of the sapphire after pre-plating for 25 s. As can be seen from the high-magnification figure in Figure 2d, enormous small particles of the Ni-P alloy are deposited on the sapphire surface in uniform distribution. Generally, the size range of Ni-P particles is between 50 nm to 100 nm. No area that is not covered with Ni-P coatings can be found even after electroless plating for only 25 s, indicating this work has a relatively fast deposition rate. The results show that by changing the pretreatment, the coating can be deposited on the sapphire substrate, and the metallization of sapphire is successfully realized.
To further explore the deposition mechanism of the sapphire metallized layer, Figure 3 is the reaction diagram simulating the Ni-P depositions on sapphire in the electroless plating solution. Under acidic conditions, the electroless nickel plating process of the phosphite ester system is basically carried out according to the following equation [21,22]. As a reducing agent, sodium hypophosphite first undergoes a dehydrogenation reaction, and the phosphorus–hydrogen bond is split to produce HPO2 ions and reducing hydrogen atoms, as shown in Equation (2). However, HPO2 will be oxidized to HPO3 due to instability, and electrons will be released at the same time according to Equation (3). The reducing hydrogen atoms are oxidized in the acid solution to generate electrons (Equation (4)). Since there are individual catalytic Pd patches on the sapphire surface, Ni2+ will accumulate on the sapphire substrates in a large amount and be reduced to metal after obtaining nickel electrons according to Equation (5). At the same time, the hypophosphite also obtains electrons and is reduced to elemental phosphorus (Equation (6)). Since metallic nickel and elemental phosphorus are produced by the reaction at the same time and then deposited on the sapphire substrates. Thus, the deposition of the Ni-P coating can be realized. Meanwhile, many bubbles were generated during the electroless plating process. These bubbles are reduced to H2 by the combination of two reducing hydrogen atoms or electrons obtained from hydrogen ions in Equations (7) and (8).
H 2 P O 2     H P O 2   +   H  
H P O 2 +   H 2 O     H 2 P O 3   +   H +   +   e
H   H +   +   e
N i 2 +   +   2 e     N i
H 2 P O 2   +   2 H +   +   e     2 H 2 O   + P
2 H +   +   2 e     H 2
H +   H   H 2

3.2. Microstructure and Wettability of Ni-P Coatings

The surface metallization on sapphire by electroless plating was successfully achieved. Figure 4a shows the surface morphology of the Ni-P coating by scanning electron microscope (SEM). No defects, including micropores, cracks and undeposit areas, can be found in the coating, which shows good quality. This coating exhibits a nodulus structure with a particle range of 0.45–0.96 µm. Figure 4b shows the cross-section topography of the Ni-P coating. The middle bright layer is the Ni-P coating with a relatively uniform thickness of 6.3 µm. Generally, this metallized layer is evenly distributed on sapphire and shows good quality.
Figure 5 shows the XRD pattern of Ni-P coating, and there is a wide peak of Ni phase at 46°. In addition, the crystallinity of this coating is 0% calculated by JADE software, indicating that this coating has an amorphous structure. Moreover, the P content of this Ni-P coating is around 13–14 wt.%. As previously reported, the lattice strain of Ni (111) grains increases when the P content in Ni-P alloy exceeds 8 wt.%, which leads to a Ni-P coating with an amorphous structure [23].
Moreover, the vital effect of depositions on sapphire is to improve its solderability. Figure 6a,b are the cross-sections of the wetting behaviors of the Sn-3 Ag solder balls on sapphire without and with metallization, respectively. According to the Young’s equation [24], the solid–liquid interaction occurring when a droplet contacts a surface is expressed by the following equation:
cos θ = γ s g γ s l γ g l
where θ is the contact angle of a smooth surface; γsg, γsl and γgl represent the interfacial tension at solid-gas, solid–liquid and gas–liquid interfaces, respectively.
Wettability is the ability of liquid solders that spread on the surface to be soldered. Many wettability studies have shown that the values of the wetting angle can indicate the degree of wettability, as shown in Table 3 [25]. The contact angle of Sn-Ag solder on a bare copper substrate is 34°, as shown in Figure 6c, which shows good wetting. The contact angle of the sapphire sample without the Ni-P coating is 125°, which exceeds 90° and exhibits unacceptable wettability for Sn-based solder balls. On the contrary, with the aid of Ni-P coatings on sapphire, the contact angle can significantly decrease to 51°, enhancing wettability.

3.3. Joining and Fracture Mechanism of Sapphire Solder Joints

Afterwards, sapphire substrates plated with Ni-P coatings were joined with bare copper sheets by a simple reflow process. Figure 7 shows the surface topography of the sapphire solder joints and the elemental distribution. The interface microstructure at the Cu/sapphire solder interfaces shows a dense structure without obvious holes and cracks. From the EDS mapping results, the bright gray stripe in the middle is the Sn-based solder, while the upper and lower substrates are copper and sapphire, respectively. Combined with the overall morphology and Ni distribution, it is found that there is an intermittent Ni-P coating between the middle layer and the sapphire, and the coating is deposited on the sapphire with good adhesion. It shows that the coating thickness decreases gradually during the reflow process, which is caused by the reaction between the Ni-P coating and the solder.
The fracture surface topography and EDS elemental distribution are shown in Figure 8. It can be seen that there is an obvious bright white curve in the middle, and shear fracture mainly occurs at the interface between the coating and the substrate. The distribution of Sn and Ni indicates that the electroless nickel plating layer is reacted by metallurgy during the joining process. It is speculated that Sn-Ni intermetallic compounds are formed, which is consistent with studies on the interfacial reaction between Ni-P coatings and Sn-based solders [26,27].
The fracture diagram of these sapphire solder joints is illustrated in Figure 9. During the connection process, the Sn-based solder reacts with the Ni-P coating to form Ni-Sn IMC layers, leading to a continuous decrease in the thickness of the Ni-P coating. When the thickness of Ni-P coating decreases to a certain value, shear fracture occurs at the coating–sapphire interface.

4. Conclusions

In this work, the sapphire substrates were successfully catalytic activated and metallized by electroless nickel plating to achieve direct joining with copper substrates via the conventional reflow process. The conclusions can be drawn as follows:
  • A proper pretreatment for sapphire substrates was proposed to successfully deposit metallization on sapphire by a simple electroless plating process. Moreover, the deposition mechanism of the metallization on sapphire was also elaborated.
  • The metallization significantly improved the wettability of the substrates as the wetting angle of the Sn-based solders on sapphire with the metallization was reduced from 125° (without metallization) to 51°.
  • The direct joining between sapphire and copper was achieved by the conventional reflow process at 250 °C and reduced pressure. The nickel atoms from the Ni-P metallization interacted with Sn atoms in the solder, resulting in the formation of Ni-Sn IMCs to achieve metallurgical bonding at the joint interfaces.

Author Contributions

Conceptualization, J.F. and L.L.; methodology, Z.L. (Zhou Luo); software, W.H.; validation, J.F., L.L. and Q.Z.; formal analysis, L.L.; investigation, Q.Z.; resources, Z.C.; data curation, J.F.; writing—original draft preparation, Z.L. (Zhenyu Liu); writing—review and editing, L.L.; visualization, Q.Z.; supervision, L.L.; project administration, X.C.; funding acquisition, L.L. All authors have read and agreed to the published version of the manuscript.

Funding

This research was funded by Wuhan University of Technology, grant number 430070. The APC was funded by Natural Science Foundation of China (62004144, 61904127). Additional thanks to the Fundamental Research Funds for the Central Universities (Grant No. 213201006, 213134005, 2042019kf0013).

Data Availability Statement

Data presented in this article are available at request from the corresponding author.

Conflicts of Interest

The authors declare no conflict of interest.

References

  1. Dobrovinskaia, E.R.; Litvinov, L.A.; Pishchik, V.V. Sapphire: Materials, Manufacturing, Applications; Springer: New York, NY, USA, 2009. [Google Scholar]
  2. Cheng, J.; Wu, J. Experimental investigation of fracture behaviors and subsurface cracks in micro-slot-grinding of monocrystalline sapphire. J. Mater. Processing Technol. 2016, 242, 160–181. [Google Scholar] [CrossRef]
  3. Mu, D.; Feng, K.; Lin, Q.; Huang, H. Low-temperature wetting of sapphire using Sn–Ti active solder alloys. Ceram. Int. 2019, 45, 22175–22182. [Google Scholar] [CrossRef]
  4. Ning, H.; Geng, Z.; Ma, J.; Huang, F.; Qian, Z.; Han, Z. Joining of sapphire and hot pressed Al2O3 using Ag70.5Cu27.5Ti2 brazing filler metal. Ceram. Int. 2003, 29, 689–694. [Google Scholar] [CrossRef]
  5. Cui, W.; Li, S.; Yan, J.; He, J.; Liu, Y. Ultrasonic-assisted brazing of sapphire with high strength Al–4.5Cu–1.5Mg alloy. Ceram. Int. 2015, 41, 8014–8022. [Google Scholar] [CrossRef]
  6. Chen, X.; Yang, J.; Huang, G.; Chen, D.; Xiang, J.; Tiantao, L.; Liu, E. Study on the metallization mechanism of sapphire by active Molybdenum-Manganese method technology. Vac. Electron. 2018, 3, 53–57. [Google Scholar]
  7. Xin, C.; Li, N.; Yan, J. Microstructural evolution in the braze joint of sapphire to Kovar alloy by Ti-Cu metallization layer. J. Mater. Processing Technol. 2017, 248, 115–122. [Google Scholar] [CrossRef]
  8. Xu, Y.; Ma, X.; Tang, H.; Yan, J. Mechanism of the interfacial reaction between sapphire and Sn-3.5Ag-4Ti solder at a low temperature in air by ultrasound. Ceram. Int. 2020, 46, 4435–4443. [Google Scholar] [CrossRef]
  9. Xu, Y.; Ma, X.; Xiu, Z.; Yan, J. Bonding and strengthening mechanism on ultrasonic-assisted soldering of sapphire using Sn-3.5Ag-4Al solder. J. Mater. Processing Technol. 2021, 288, 116893. [Google Scholar] [CrossRef]
  10. Loto, C.A. Electroless Nickel Plating—A Review. Silicon 2016, 8, 177–186. [Google Scholar] [CrossRef]
  11. Qin, T.; Ma, L.; Yao, Y.; Ni, C.; Ding, Y. An in situ measure method to study deposition mechanism of electroless Ni-P plating on AZ31 magnesium alloy. Trans. Nonferrous Met. Soc. China 2011, 21, 2790–2797. [Google Scholar] [CrossRef]
  12. Wang, M.; Yang, Z.; Zhang, C.; Liu, D. Growing process and reaction mechanism of electroless Ni–Mo–P film on SiO2 substrate. Trans. Nonferrous Met. Soc. China 2013, 23, 3629–3633. [Google Scholar] [CrossRef]
  13. Georgiza, E.; Novakovic, J.; Vassiliou, P. Characterization and corrosion resistance of duplex electroless Ni-P composite coatings on magnesium alloy. Surf. Coat. Technol. 2013, 232, 432–439. [Google Scholar] [CrossRef]
  14. Wei, Y.; Li, Y.; Zhang, Y.; Luo, X.; Li, C. Corrosion resistant nickel coating with strong adhesion on AZ31B magnesium alloy prepared by an in-situ shot-peening-assisted cold spray. Corros. Sci. 2018, 138, 105–115. [Google Scholar] [CrossRef]
  15. Guo, X.; Du, K.; Guo, Q.; Wang, Y.; Wang, F. Experimental study of corrosion protection of a three-layer film on AZ31B Mg alloy. Corros. Sci. 2012, 65, 367–375. [Google Scholar] [CrossRef]
  16. Shang, W.; Zhan, X.; Wen, Y.; Li, Y.; Wang, C. Deposition mechanism of electroless nickel plating of composite coatings on magnesium alloy. Chem. Eng. Sci. 2019, 207, 1299–1308. [Google Scholar] [CrossRef]
  17. Zhang, P.; Lv, Z.; Liu, X.; Xie, G.; Zhang, B. Electroless nickel plating on alumina ceramic activated by metallic nickel as electrocatalyst for oxygen evolution reaction. Catal. Commun. 2021, 149, 106238. [Google Scholar] [CrossRef]
  18. Dehchar, C.; Chikouche, I.; Kherrat, R.; Sahari, A.; Zouaoui, A.; Merati, A. Electroless copper deposition on epoxy glass substrate for electrocatalysis of formaldehyde. Mater. Lett. 2018, 228, 439–442. [Google Scholar] [CrossRef]
  19. Hui, Z.; Huang, Z.; Cui, J. A new method for electroless Ni–P plating on AZ31 magnesium alloy. Surf. Coat. Technol. 2007, 202, 133–139. [Google Scholar]
  20. Ranjbar, M.; Garavand, N.; Mahdavi, S.; Zad, A. Electroless plating of palladium on WO3 films for gasochromic applications. Sol. Energy Mater. Sol. Cells 2010, 94, 201–206. [Google Scholar] [CrossRef]
  21. Zhang, B. Mechanism of Electroless Plating. Amorph. Nano Alloy. Electroless Depos. 2016, 4, 583–627. [Google Scholar]
  22. Lin, J.; Chou, C. The influence of phosphorus content on the microstructure and specific capacitance of etched electroless Ni-P coatings. Surf. Coat. Technol. 2019, 368, 126–137. [Google Scholar] [CrossRef]
  23. Lewis, D.B.; Marshall, G.W. Investigation into the structure of electrodeposited nickel-phosphorus alloy deposits. Surf. Coat. Technol. 1996, 78, 150–156. [Google Scholar] [CrossRef]
  24. Liu, Y.; Shi, J.; Lu, Q.; Guo, Y.; Chen, R.; Yin, D. Survey on Calculation of Solid Surface Tension Based on Young’s Equation. Mater. Rev. 2013, 27, 123–129. [Google Scholar]
  25. Moser, Z.; Gąsior, W.; Pstruś, J.; Dębski, A. Wettability Studies of Pb-Free Soldering Materials. Int. J. Thermophys. 2008, 29, 1974–1986. [Google Scholar] [CrossRef]
  26. Kumar, A.; Min, H.; Zhong, C. Barrier properties of thin Au/Ni–P under bump metallization for Sn–3.5Ag solder. Surf. Coat. Technol. 2005, 198, 283–286. [Google Scholar] [CrossRef]
  27. Yang, Y.; Yang, C.; Ouyang, F. Interfacial reaction of Ni3Sn4 intermetallic compound in Ni/SnAg solder/Ni system under thermomigration. J. Alloy. Compd. 2016, 674, 331–340. [Google Scholar] [CrossRef]
Figure 1. Macroscopic appearance of samples.
Figure 1. Macroscopic appearance of samples.
Materials 15 01783 g001
Figure 2. Topography of the substrate in electroless plating pretreatment after (a) grinding, (b) etching, (c) activation and (d) initial plating.
Figure 2. Topography of the substrate in electroless plating pretreatment after (a) grinding, (b) etching, (c) activation and (d) initial plating.
Materials 15 01783 g002
Figure 3. Deposition process and mechanism in the electroless plating solution.
Figure 3. Deposition process and mechanism in the electroless plating solution.
Materials 15 01783 g003
Figure 4. (a) Surface morphology, (b) section morphology of Ni-P coating.
Figure 4. (a) Surface morphology, (b) section morphology of Ni-P coating.
Materials 15 01783 g004
Figure 5. XRD pattern of Ni-P coating.
Figure 5. XRD pattern of Ni-P coating.
Materials 15 01783 g005
Figure 6. Wetting angles of Sn-Ag solder balls on (a) bare sapphire, (b) Ni-P plated sapphire and (c) bare Cu substrate.
Figure 6. Wetting angles of Sn-Ag solder balls on (a) bare sapphire, (b) Ni-P plated sapphire and (c) bare Cu substrate.
Materials 15 01783 g006
Figure 7. Morphology and EDS elemental distribution at Cu/sapphire solder interfaces.
Figure 7. Morphology and EDS elemental distribution at Cu/sapphire solder interfaces.
Materials 15 01783 g007
Figure 8. Element analysis diagram of fracture surface morphology.
Figure 8. Element analysis diagram of fracture surface morphology.
Materials 15 01783 g008
Figure 9. Cu/solder/sapphire fracture schematic diagram.
Figure 9. Cu/solder/sapphire fracture schematic diagram.
Materials 15 01783 g009
Table 1. Studies on metallization methods on sapphire.
Table 1. Studies on metallization methods on sapphire.
MethodsTemperatureConditionsDisadvantageReference
Mo-Mn sintering950~1000 °CReducing atmospherePore and microcrack defects[6]
Magnetron sputtering<50 °CVacuum conditionHigh cost, low material utilization[7]
Ultrasonic assisted hot dipping210~230 °CActive solders (Ti, Al, Mg)Ultrasonic damage[8,9]
Table 2. Chemical plating bath composition and conditions.
Table 2. Chemical plating bath composition and conditions.
Chemical ReagentsComposition (g/L)
NiSO4·6H2020–35
NaH2PO·2H2O25–35
Na3C6H5O7·2H2O60–70
((NH4)2SO460–80
Plating conditionTemp: 65–75 °C, pH: 5–6, Time: 15–30 min
Table 3. The correlation of wetting angle range with wettability.
Table 3. The correlation of wetting angle range with wettability.
Wetting Angle RangeWettability
0° ≤ θ < 30°Excellent wetting
30° ≤ θ < 40°Good wetting
40° ≤ θ < 55°Acceptable wetting
55° < θ < 70°poor wetting
70° ≤ θUnacceptable wetting
Publisher’s Note: MDPI stays neutral with regard to jurisdictional claims in published maps and institutional affiliations.

Share and Cite

MDPI and ACS Style

Fang, J.; Zhang, Q.; Luo, Z.; Huang, W.; Liu, Z.; Chen, Z.; Cao, X.; Liu, L. Metallization on Sapphire and Low-Temperature Joining with Metal Substrates. Materials 2022, 15, 1783. https://doi.org/10.3390/ma15051783

AMA Style

Fang J, Zhang Q, Luo Z, Huang W, Liu Z, Chen Z, Cao X, Liu L. Metallization on Sapphire and Low-Temperature Joining with Metal Substrates. Materials. 2022; 15(5):1783. https://doi.org/10.3390/ma15051783

Chicago/Turabian Style

Fang, Jiajun, Qiaoxin Zhang, Zhou Luo, Wei Huang, Zhenyu Liu, Zhiwen Chen, Xueqiang Cao, and Li Liu. 2022. "Metallization on Sapphire and Low-Temperature Joining with Metal Substrates" Materials 15, no. 5: 1783. https://doi.org/10.3390/ma15051783

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.