Article

Properties of Rubberized Engineered Cementitious Composites Containing Nano-Silica

by
Rubendran Loganathan
and
Bashar S. Mohammed
*
Department of Civil and Environmental Engineering, Universiti Teknologi PETRONAS (UTP), Bandar Seri Iskandar 32610, Perak, Malaysia
*
Author to whom correspondence should be addressed.
Materials 2021, 14(13), 3765; https://doi.org/10.3390/ma14133765
Submission received: 6 May 2021 / Revised: 24 May 2021 / Accepted: 3 June 2021 / Published: 5 July 2021

Abstract

:
To avoid explosive spalling during elevated temperature, crumb rubber (CR) is being added to the manufacturing of engineered cementitious composites (ECC). However, the addition of CR particles adversely affects the mechanical properties of ECC. Therefore, to overcome this issue, nano-silica (NS) is added into rubberized ECC mixture as cementitious material additives. Response surface methodology (RSM) has been utilized to optimize the mixtures of the rubberized ECC with variables: CR (0, 2.5, and 5 vol.%), polyvinyl alcohol (PVA) fiber (0, 1, and 2 vol.%), NS (0, 1, and 2 vol.%), and fly ash (0, 25, and 50 vol.%). The experimentally measured responses are flexural strength, direct tensile strength, elastic modulus, Poisson’s ratio, creep, and drying shrinkage. Mathematical models to predict the targeted responses have been developed using RSM. As a result, a high correlation between the factors and responses has been exhibited by the developed models and the accuracy of fit, where less than 9.38% of the variation was found between the predicted and validated results. The experimental results revealed that the rubberized ECC with the incorporation of nano-silica exhibited a higher compressive strength, direct tensile strength, flexural strength, elastic modulus, Poisson’s ratio, and lower drying shrinkage.

1. Introduction

Scrap tires are one of the world’s largest solid wastes and more than 500 million units of waste tires are deposited each year before any type of treatment [1]. In Malaysia, the amount of annually produced scrap tires is in the range of 8.2 million tons, and about 60% of the scrap tires are deposited through unknown channels [2,3]. Most of these scrap tires are generally substantial, bulky and occupy unnecessary space in landfills. The accumulation of scrap tires in abandoned places is a perfect area for a breeding floor for mosquitoes and pests, which, in turn, can be deadly to humans. Additionally, scrap tires are also known to be a non-biodegradable item [4,5]. One solution to counteract this environmental problem is by incorporating crumb rubber (CR) from scrap tires into the production of construction and building materials, such as concrete [6]. CR is defined as the end product of rubber that has been recycled from vehicle tires [7].
Mohammed et al. [8] confirmed that the utilization of CR in concrete as a partial replacement to fine aggregate by volume has led to improve the properties of concrete, which has been named “rubbercrete”. As compared to normal concrete, rubbercrete shows better acoustic properties [9], lower thermal conductivity [10], higher electrical resistivity [11], and more ductility [12], as well as a lower self-weight (own weight of body, due to the mass present in it) [13]. However, as the percentage of CR increases, the strengths (compressive, tensile, and flexural) and elastic modulus of rubbercrete decreases [14,15]. This is attributed to the hydrophobic nature of the CR particles, which repel water and entraps air on their surface [10,11,15,16]. This is the main reason why the interfacial transition zone (ITZ) between CR particles and the hardened cement matrix becomes thicker and weaker [10], which consequently leads to a reduction in the strength of rubbercrete [14]. Thus, researchers have attempted to resolve the problem of the reduction in strengths of rubbercrete using several methods. The widely used methods to restore the lost strength is either through surface treatment of the crumb rubber before mixing with concrete or by the inclusion of cementitious additives into the concrete [17]. One of the additives is nano-silica (NS), which has been utilized in the production of rubbercrete, and its primary purpose is to enhance and restore the strength of rubbercrete through dual physico-chemical functions. Through the chemical process, nano-silica reacts with calcium hydroxide, which is discharged by the hydration process from the cement and subsequently cultivates the production of calcium silicate hydrate (C–S–H) gel which restores strength. In the physical process, nano-silica also acts as a nanofiller. Both functions of NS lead to densifying the microstructure of the hardened cement matrix and the ITZ [8].
On the other hand, engineered cementitious composite (ECC) is a distinctive type of high-performance, fiber-reinforced cementitious composite (HPFRCC) in accordance with the micromechanics principle and the mechanics of fracture [18]. ECC possesses multiple cracks whereas the width openings of the cracks are generally less than 100 μm [19]. As is well documented in the literature, ECC exhibits tensile strength within the range of 4–6 MPa, a compression strain of 0.4–0.65% [3], and compressive strength in the range of 30–80 MPa [20].
Despite the advantages of ECC, its main drawback is explosive spalling when it is being subjected to rapid elevated temperature during fires [21,22,23]. Under a fire situation, the entrapped water and chemically bound water evaporate. Due to the highly densified and disconnected pore system of the ECC, the internal vapor is entrapped in the ECC and will not find its way out [24]. This leads to a high internal pressure build up, followed by explosive spalling [25]. To ease this problem, researchers have incorporated CR in the ECC mixture to avoid explosive spalling in case of a fire. As the CR particles in the ECC would melt under the heat, the residue would connect the pores and consequently provide a passage for vapor to escape. However, by adding crumb rubber to ECC, it could facilitate this situation and explosive spalling would not occur; however, at the same time, to maintain the strength of the ECC, nano-silica has been included to overcome the reduction in ECC strength as well as of the modulus elasticity (ME).
The inclusion of CR into concrete had attracted plenty of attention in the construction industry with regards to how building materials are prepared. As previously mentioned, the innovative aspects of this study, which include CR particles into ECC, could solve a fundamental problem pertaining to when samples encounter fire. This solution would, not only be beneficial to the way building materials are utilized, but also further research could be done on a larger scale.

2. Experimental Program

2.1. Material Properties

The cementitious material used in preparation of the ECC mixtures were ordinary Portland cement (OPC, Tasek Corporation Berhad, Ipoh, Perak, Malaysia), fly ash (FA, YTL Cement Berhad, Kuala Lumpur, Malaysia), and nano-silica (NS, Zhengzhou Dongshen Petrochemical Technology, China). The OPC (Type 1) and class F FA conform to the requirements of ASTM C150 [26] and ASTM C618 [27], respectively; the chemical and physical properties are shown in Table 1. The properties of the nano-silica are shown in Table 2. River sand (Tronoh, Perak, Malaysia) with a specific gravity of 2.65 g/cm3, fineness modulus of 2.86, and water absorption of 1.24% was utilized as a fine aggregate in accordance with the requirements of ASTM C33. Untreated Mesh 30 crumb rubber (CR, Heap Hoe Tyres Sdn Bhd, Kedah, Malaysia) with a specific gravity of 0.95 g/cm3 was used as a partial replacement to sand by volume. The gradation curves for fine aggregates and crumb rubber are shown in Figure 1, which were determined in accordance with the requirements of ASTM C136/C136M-14 [28].
PVA fibers (12 mm long and 40 μm circular cross-sectional diameter, (Kuraray, Okayama, Japan) were used as the primary reinforcement for the rubberized ECC mixture; the physical properties of the PVA fibers are shown in Table 3. Polycarboxylate based superplasticizers (Sika Viscocrete-2044, Sika Kimia Sdn Bhd, Negeri Sembilan, Malaysia) with a pH value of 6.2, specific gravity of 1.08 g/cm3, an absence of chloride ion content, and a density of 1.11 kg/L were used to achieve the desired flowability for all mixtures, as the water content was kept constant. Based on trial and errors mixtures, the water-cement ratio was limited to 0.15 in the rubberized ECC mixture to avoid bleeding and segregation, as well as to ensure paste workability to achieve the target compressive strength of 73.5 MPa.

2.2. Rubberized ECC Mixtures Proportions Using RSM

Response surface methodology (RSM) is the most adequate computational and mathematical approach used and is most widely used for the analysis and design of models that relate and respond to one or more independent factors. RSM also used to optimize models with multiple objectives by specifying desirable objectives according to responses or factors [29,30]. Various design forms, including central composite, Box-Behnken, and historical data, are usable for RSM analyses, which might be utilized to establish statistical relationships between responses and independent factors. The selection of a design model is based on several responses and factors [30].
In this study, Design Expert software (Design Expert v10, StatEase, Godward, MN, USA) was used for RSM optimization and the mixtures proportions. The central composite design (CCD) approach was used for designing the experiments based on four factors, namely CR, fly ash, PVA, and NS. Three variations of CR were used as partial replacements to fine aggregates (0, 2.5, and 5% by volume) and fly ash was used as a partial replacement to cement (OPC) (0, 25 and 50% by weight). As for the addition of nano-silica and PVA fiber, the variations were 0, 1, and 2% by weight of cementitious material. A total of 30 trial mix designs, along with their proportions, were then produced using RSM. For each mix, the water-cement ratio was kept constant at a value of 0.15. For each mix, the flexural strength, direct tensile strength, elastic modulus, Poisson’s ratio, creep, and drying shrinkage were tested in a lab, and were considered as the responses for RSM analyses and mixture optimizations. The best mix design and optimization model were then determined. The total mixture constituents are depicted in Table 4.

2.3. Specimens Preparation and Test Procedures

Each mixture was prepared in the following order: the ingredients were first weighed with a weighing scale, then the dry materials of cement, fine aggregates, crumb rubber and fly ash were mixed under dry conditions using a pan type concrete mixer (UTEST, Ankara, Turkey) with continuous stirring for about 1–2 min. Water and superplasticizer were then slowly added and the mixing continued for another 5 min. At this stage, after one minute, the nano-silica and PVA were added. PVA fibers were added gradually to avoid balling effects and then mixing continued for another 2–3 min. After measuring the flowability of the mixture, the molds were prepared according to each testing standard and then kept in a curing room for 24 h. Samples were then demolded and kept in a curing water tank at 23 °C until a testing age of 28 days of curing.
Compressive strength tests were conducted in accordance with requirements of ASTM C109/C109M [31]. Three 50-mm cubic samples were tested at 28 days using a 3000kN capacity digital Universal Testing Machine (UTM, ELE, Leighton Buzzard, UK).
The direct tensile strength was carried out on dog-boned-shaped samples using a uniaxial tensile testing machine (GOTECH, Taichung City, Taiwan), as shown in Figure 2a,b, in accordance with the requirements and recommendations of Rokugo [32]. A total of 3 specimens for each mix was prepared and tested at 28 days of curing. The gauge length of the specimens was 80 mm and loading were applied at a controlled displacement rate of 0.005 mm/s. The load and displacement values were measured using a longitudinal potential displacement transducer (LPDT, GOTECH, Taichung City, Taiwan) that was built into the machine and the measurements were captured using a computer data recording system (U60 v6.1 Software, Gotech Testing Machines Inc, Taichung City, Taiwan).
For the flexural strength test, a 200kN capacity digital Universal Testing Machine (UTM, GOTECH, Taichung City, Taiwan), three beams per mix, with dimensions of 500 mm × 100 mm × 25 mm, as shown in Figure 2c, were prepared and tested under a three-point bending test in accordance with the requirements of ASTM C293/C293M [33] at a uniform rate of stress 0.06 MPa/s.
The elastic modulus and Poisson’s ratio of rubberized ECC were measured using testing cylinder samples with a 150 mm diameter and 300 mm height at 28 days in accordance with the requirements of ASTM C469/C469M-14 [34] (as shown in Figure 2d). The 3000kN capacity digital Universal Testing Machine (UTM, ELE, Leighton Buzzard, UK) was fitted with a longitudinal compressometer to measure the vertical strain and an extensometer to measure the lateral strain. To measure the Poisson’s ratio, a load was applied to the specimens at a rate of 35 ± 5/s psi. The applied load and its corresponding deformation were recorded. In addition, when the applied load has reached 40% of the ultimate load, the elastic modulus can then be calculated.
For the creep test, once the optimized mix proportions were obtained, six cylindrical specimens (150 mm × 300 mm) were prepared in accordance with the requirements of ASTM C512/C512M-15 [35]. Two samples were used for compressive strength and the remaining four samples were used for the creep test. After casting, the specimens were stored in a curing room at a temperature of approximately 23 °C for 24 h, then demolded and cured in a clean water tank at 23 °C for 7 days. Four demountable mechanical (DEMEC) gauge points were attached, i.e., two on each diametrically opposing side at 200 mm, as shown in Figure 3a. Two spring loaded loading frames (Wuxi, China) were used and comprised four vertical threaded shafts. Four springs are attached at the lower ends of the shafts, sandwiched between two bearing plates (upper base plate and lower base plate), as shown in Figure 3b. The springs were connected for the application and maintained the applied loads within a scope of ±2% in the event of any change in the dimensions of the specimens. Loading was applied by means of a hydraulic pump, two jack plates (upper and lower), which were spaced at a distance that could be adjusted depending on the size of the hydraulic jack pump. To prevent eccentricity in the samples, two loading plates were attached to ensure the specimens could be positioned on the loading frame without much movement. The distance between loading frames did not exceed 1780 mm. Finally, to achieve a smooth surface for the specimens and to promote uniform distribution of stresses, the bottom and top of each sample were capped using a two-part epoxy resin, Sikadur -330 where it was prepared by mixing (component A) with a hardener (component B) at a weight ratio of 4:1. For each mix, the specimens were connected (top to bottom) with the epoxy resin before the plugs were placed. The whole assembly was then placed and aligned into the creep loading frame, as shown in Figure 3b. Creep was calculated using Equation (1), and the coefficient of creep was calculated using Equation (2).
C t k , t 0 = ε t t k     ε i e t 0     ε s h t k
ϕ t k ,   t 0 = C t k , t 0 ε i e t 0
where C t k , t 0   is total creep at time t k due to the applied stress at time t 0 ; ε t t k is total strain at time t k ; ε i e t 0   is initial instantaneous elastic strain at time t 0 ; ε s h t k is corresponding shrinkage strain for the same specimen at time t k ; and ϕ t k ,   t 0   is creep coefficient at any time, t k .
Finally, the drying shrinkage was carried out with prisms with dimensions of 75 mm × 75 mm × 300 mm. Shrinkage deformation was determined by the change in length of the specimens (difference in initial length and final length after air-drying age of 28 days). A total of three specimens for each mixture were tested with accordance with ASTM C490/C490M-17 [36].

3. Results and Discussions

3.1. Creep Test Results

The creep measurement for the ECC mixtures were reported in two forms, total creep strain and creep coefficients, as shown in Figure 4. Both ECC mixtures show an increase in creep strain and creep coefficient over time. The rate of increase was higher in the early stages and gradually followed a steady incline throughout the rest of the testing period. This was bound to happen, as during the early stages of concrete, the compressive strength of concrete is very low, and thus, deformation could occur a great deal easier when loading is applied. In addition, as time continues, the hydration of cement takes place, which, in turn, results in the ECC gaining strength, which also, in turn, increases the elastic modulus and consequently reduces deformation under the long duration of applied loading. The addition of nano-silica decreased the overall creep strain and creep coefficient for both ECC mixtures. When comparisons were made, the total creep of M2 to M1 showed higher percentages, by 17.64, 68.6, 22.24% at the 7th, 30th and 90th days, respectively. The creep coefficient, on the other hand, for M1, ranged from 0.225 to 0.415, whereas, for M2, it ranged from 0.234 to 0.555. It is noticeable that there was a slight difference between the creep coefficient ranges between M1 and M2, and this was attributed to the fact that, when crumb rubber was added (lower stiffness compared to fine aggregates), it lowered the overall creep of the ECC. M1 and M2 had equal amounts of crumb rubber added into the mixture, hence, justifying the similarities in terms of ranges for creep coefficients of M1 and M2.

3.2. Response Surface Methodology (RSM)

RSM is the most adequate computational and mathematical approach used and the most widely used for analyses and the design of models that relate and respond to one or more independent factors [37]. The analysis of RSM involves developing a sequence of tests and gathering the experimental outcomes as answers. The operation is launched using response surface modeling, in which the central composite design (CCD) model was selected to suit the information set. For each variable, three levels of study were considered, at low, medium, and high levels. This was to provide an overall response at only one center point. The experimental design matrix and the experimental results are shown in Table 5.

3.3. Analysis of Variance (ANOVA)

Table 6 shows that the analysis of variance (ANOVA) results for the quadratic response models demonstrate significant ability of the developed models in estimating the properties of rubberized ECC containing nano-silica. The models’ F-values of 16.36, 3.15, 16.31, 5.28, 61.52, and 3.15, for compressive strength, elastic modulus, Poisson’s ratio, direct tensile strength, drying shrinkage, and flexural strength, respectively, indicated that the models were all significant, with only a 0.01% probability value (p-value) for all models. The significance of all factors, including models and their terms, could be examined using a 95% of confidence level (CI), where the p-value should be less than 0.05. For compressive strength, the model and the terms A, B, C, AB, BD, B2, and D2 were all significant as their p-values were less than 0.05, whereas, the p-values for the terms D, AC, AD, BC, CD, A2, and C2 were greater than 0.05, which means they are all not significant. For elastic modulus, the model and its terms A, B2, C2, and D2 were significant because they had p-value < 0.05 , but the rest of the model terms (B, C, D, A2, AB, AC, AD, BC, BD, and CD) were insignificant due to the p-value being > 0.05 . For the Poisson’s ratio, the model and terms A, C, D, C2, AD, BD, and CD were significant, while the model terms B, A2, B2, C2, D2, AB, AC, and BC were not significant with p-values of > 0.05 . For the direct tensile strength, the model and terms C, D, AD, BD, and D2 had p-values less than 0.05, which were significant, while the remaining models’ terms were insignificant. For the drying shrinkage model, only terms A, C, D, AC, CD, A2, and D2 were significant with p-values < 0.05 , whereas the rest of its terms were insignificant, with p-values > 0.05 . Finally, only four models’ terms of flexural strength A, B2, C2, and D2 were significant while the remaining ten terms were not significant with p-values > 0.05 . Based on ANOVA analysis, the proposed models that were created using Design Expert software assumed quadratic models and the empirical interactions between each input factor and output factor are as shown in Equations (3)–(8) (for compressive strength (CS), elastic modulus (EM), Poisson’s ratio ( v ), direct tensile strength (DT), drying shrinkage (DS), and flexural strength (FS), respectively). The positive and negative symbols before the model term represent antagonistic and synergistic effects of the independent factors on the responses of rubberized ECC.
C S   M P a = 65.14 15.56 A 3.29 B 2.77 C + 0.62 D + 3.89 A * B + 0.76 A * C 0.84 A * D + 1.97 B * C + 4.59 B * D + 0.626 C * D + 0.045 A 2 7.66 B 2 4.74 C 2 + 14.76 D 2
E M   M P a = 25.08 2.13 A + 0.61 B + 0.45 C 0.104 D 0.59 A * B 0.03 A * C 0.51 A * D 0.32 B * C 0.46 B * D 0.43 C * D 0.019 A 2 4.66 B 2 + 4.33 C 2 3.18 D 2
v = 0.25 0.029 A 0.0016 B 0.01 C 0.013 D + 0.0016 A * B 0.0044 A * C + 0.027 A * D + 0.0045 B * C 0.0079 B * D 0.011 C * D 0.0097 A 2 + 0.01 B 2 + 0.02 C 2 0.0062 D 2
D T   M P a = 2.74 0.019 A 0.021 B + 0.13 C + 0.15 D 0.076 A * B + 0.014 A * C + 0.266 A * D 0.0099 B * C + 0.15 B * D + 0.01 C * D 0.063 A 2 + 0.076 B 2 + 0.071 C 2 + 0.337 D 2
DS   µ E = 1274 + 110.1 A + 6.68 B 8.3 C + 8.9 D 2.66 A * B + 13.14 A * C 0.102 A * D + 3.01 B * C 2.01 B * D + 13.41 C * D 64.6 A 2 + 4.37 B 2 1.1 C 2 + 89.73 D 2
F S   M P a = 10.5 + 0.54 A + 0.041 B 0.027 C + 0.524 D 0.038 A * B 0.048 A * C 0.138 A * D 0.231 B * C 0.133 B * D 0.03 C * D 1.31 A 2 + 0.113 B 2 0.011 C 2 + 0.803 D 2
The developed models presented in Equations (3)–(8) showed insignificant terms (p-value > 0.05) which meant that these terms should be omitted from the equations. Therefore, the final models after removing all insignificant terms are presented as Equations (9)–(14), for compressive strength (CS), elastic modulus (EM), Poisson’s ratio ( v ), direct tensile strength (DT), drying shrinkage (DS), and flexural strength (FS), respectively.
C S   M P a = 65.14 15.56 A 3.29 B 2.77 C + 3.89 A * B + 4.59 B * D 7.66 B 2 + 14.76 D 2
E M   M P a = 25.08 2.13 A 4.66 B 2 + 4.33 C 2 3.18 D 2
v = 0.25 0.029 A 0.01 C 0.013 D + 0.027 A * D 0.0079 B * D 0.011 C * D
D T   M P a = 2.74 + 0.13 C + 0.15 D + 0.266 A * D + 0.15 B * D + 0.337 D 2
DS   µ E = 1274 + 110.1 A 8.3 C + 8.9 D + 13.14 A * C + 13.41 C * D 64.6 A 2 + 89.73 D 2
F S   M P a = 10.46 + 0.54 A + 0.11 B 2 0.011 C 2 + 0.803 D 2
To confirm the adequacy, fitness, and consistency of these models, a degree of determination (correlation) was used. Table 6 shows a summary of the response model validation. The R2 values were significant for all models, which were greater than 90% (R2 > 0.9). The high values of the determination coefficient of R2 symbolized a good agreement between the determined responses to the proposed models in estimating the properties of rubberized ECC containing nano-silica. Consequently, all models were statistically satisfactory. Adequate precision (AP) was also determined to measure the ratio of signal to noise where every response was more significant than the desired value, as the AP value for all models was greater than 4. Furthermore, all models’ variabilities were also tested using their standard deviations (S.D.) and coefficients of variation (C.V.) with reference to the experimental results. In addition to the mean (μ) of the models, the low S.D. values revealed that the experimental results were more correlated to the developed models, which mean both results fit. Therefore, it could be concluded that the developed models can be employed to command the design space as seen in Table 7.
Figure 5, Figure 6, Figure 7 and Figure 8 show the 3D response surface plots for compressive strength, flexural strength, direct tensile strength, elastic modulus, Poisson’s ratio, and drying shrinkage of rubberized ECC. As shown in Figure 5, the compressive strength, flexural strength, direct tensile strength, and elastic modulus of the rubberized ECC decreases with increasing crumb rubber content. This reduction is attributed to the hydrophobic nature of crumb rubber, which repels water and entraps air on its surface leading to increasing air voids inside the hardened ECC cement matrix, which thickens and weaken the interfacial transition zone (ITZ) between the CR particles and the hardened cement matrix. However, adding nano-silica to the mixture leads to an increase in compressive strength, flexural strength, direct tensile strength, and elastic modulus of the rubberized ECC due to the pozzolanic reaction of nano-silica with surplus Ca(OH)2 from cement hydration and produces more calcium-silicate-hydrate (C–S–H) gel, resulting in increased strength through densification of the microstructure of the hardened cement matrix and also the ITZ. On the other hand, Figure 6 shows that the Poisson’s ratio decreases, and the drying shrinkage increases with increasing CR content. It also shows that the addition of nano-silica increases the Poisson’s ratio and decreases the drying shrinkage due to the reduction of the permeability because of the formation of secondary C–S–H from the high pozzolanic reaction of nano-silica. The formed C–S–H gel fills up the capillary pores in the rubberized ECC matrix and thus reduces drying shrinkage.

3.4. Multi-Objective Optimization

The optimization process aimed to identify the optimum values (factors proportion) using the response surface of the chosen model to accomplish an optimized rubberized ECC mix. To acquire all the different combinations of outcomes, all factors were defined in the optimization criteria and a target compressive strength of 50 MPa was chosen; the responses were either maximized or minimized, as shown in Table 8. The creep test response was not included in the multi-objective optimization as it was conducted after the optimized rubberized ECC mixtures were obtained. The resulting optimized mix proportions were then used to conduct the creep test. By utilizing RSM using the Design Expert software, the optimization process and the desirability function were carried out. To validate each optimized rubberized ECC mixture, as well as to obtain a consistent result that was not altered by random events, the first three outcomes with the highest desirability value of 1 were chosen.
Table 9 presents the selected multi-objective optimization results of the rubberized ECC mixtures that gave a desirability of 1. The optimized mixture of rubberized ECC containing nano-silica was accomplished via partial substitution of fine aggregates with crumb rubber at 3.4% by volume and replacing 42.14% of the cement with fly ash by volume, as well as the addition of 1.345% and 1.245% of nano-silica and PVA fibers by weight of cementitious materials, respectively. The optimized outcome had a desirability of 1.0%. The corresponding results of the optimized mix for all the responses are shown in Table 9.

3.5. Model Validation

The optimized results and all model responses were then validated via experimental works, and the average results were compared to determine the percentage error for both experimental and optimized values (predicted). Table 10 shows the percentage difference between the experimental and predicted model results. The maximum percentage error across every response was 9.38%, which validated a good correspondence of the experimental, as well as the optimized results. This indicated that the proposed model for this research using RSM is highly reliable and can be used to predict the properties of rubberized ECC containing nano-silica.

4. Conclusions

Based on the results of the experimental and statistical analyses, the following conclusions can be drawn:
  • Incorporation of nano-silica can offset the adverse effects of crumb rubber content on the properties of rubberized ECC.
  • The reduction in the elastic modulus of rubberized ECC is attributed to the elastic properties of the crumb rubber particles, which act as tiny springs inside the hardened cement matrix. However, this adverse effect has been offset by adding nano-silica which restricted the internal structure of the rubberized ECC.
  • The developed quadratic equations can be used to predict the responses. All the responses are within the 5% significance level, where the probability value (p-value) is less than 0.05, clearly indicating that the models are significant with an outstanding 95% confidence level. The developed models using the RSM can provide reliable and accurate responses and thus can be used to predict the strength of the rubberized ECC containing NS.
  • The optimum mixture of rubberized ECC mixture achieved using RSM is highly reliable.

Author Contributions

Conceptualization, R.L. and B.S.M.; methodology, R.L. and B.S.M.; software, R.L.; validation, R.L.; formal analysis, R.L. and B.S.M.; investigation, R.L.; resources, B.S.M.; writing—original draft preparation, R.L.; writing—review and editing, B.S.M.; supervision, B.S.M.; project administration, B.S.M.; funding acquisition, B.S.M. All authors have read and agreed to the published version of the manuscript.

Funding

The authors would like to thank Universiti Teknologi Petronas (UTP) Malaysia for supporting and funding projects 015LC0–097 and 015ME0-125.

Institutional Review Board Statement

Not applicable.

Informed Consent Statement

Not applicable.

Data Availability Statement

The data used to support the findings of this study are included within the article.

Conflicts of Interest

The authors declare no conflict of interest.

References

  1. Thomas, B.S.; Gupta, R.C.; Panicker, V.J. Recycling of waste tire rubber as aggregate in concrete: Durability-related performance. J. Clean. Prod. 2016, 112, 504–513. [Google Scholar] [CrossRef]
  2. Kumar, T. Waste Tyre Management in Malaysia. Ph.D. Thesis, Putra University, Seri Kembangan, Malaysia, 2006. [Google Scholar]
  3. Al-Fakih, A.; Mohammed, B.S.; Liew, M.S.; Alaloul, W.S.; Adamu, M.; Khed, V.C.; Dahim, M.A.; Al-Mattarneh, H. Mechanical behavior of rubberized interlocking bricks for masonry structural applications. Int. J. Civ. Eng. Technol. 2018, 9, 185–193. [Google Scholar]
  4. Bulei, C.; Todor, M.; Heput, T.; Kiss, I. Directions for material recovery of used tires and their use in the production of new products intended for the industry of civil construction and pavements. In IOP Conference Series: Materials Science and Engineering; IOP Publishing: Bristol, UK, 2018; p. 012064. [Google Scholar]
  5. Al-Fakih, A.; Mohammed, B.S.; Liew, M.S.; Alaloul, W.S. Physical properties of the rubberized interlocking masonry brick. Int. J. Civ. Eng. Technol. 2018, 9, 656–664. [Google Scholar]
  6. Mohammed, B.S. Structural behavior and m–k value of composite slab utilizing concrete containing crumb rubber. Constr. Build. Mater. 2010, 24, 1214–1221. [Google Scholar] [CrossRef]
  7. Khan, S.; Singh, A. Behavior of Crumb Rubber Concrete. Int. J. Res. Eng. 2018, 8, 86–92. [Google Scholar]
  8. Mohammed, B.S.; Awang, A.B.; Wong, S.S.; Nhavene, C.P. Properties of nano silica modified rubbercrete. J. Clean. Prod. 2016, 119, 66–75. [Google Scholar] [CrossRef]
  9. Li, G.; Garrick, G.; Eggers, J.; Abadie, C.; Stubblefield, M.A.; Pang, S.-S. Waste tire fiber modified concrete. Compos. Part B Eng. 2004, 35, 305–312. [Google Scholar] [CrossRef]
  10. Mohammed, B.S.; Anwar Hossain, K.M.; Eng Swee, J.T.; Wong, G.; Abdullahi, M. Properties of crumb rubber hollow concrete block. J. Clean. Prod. 2012, 23, 57–67. [Google Scholar] [CrossRef]
  11. Onuaguluchi, O.; Panesar, D.K. Hardened properties of concrete mixtures containing pre-coated crumb rubber and silica fume. J. Cleaner Prod. 2014, 82, 125–131. [Google Scholar] [CrossRef]
  12. Shu, X.; Huang, B. Recycling of waste tire rubber in asphalt and portland cement concrete: An overview. Constr. Build. Mater. 2014, 67, 217–224. [Google Scholar] [CrossRef]
  13. Demir, F.; Yesilata, B.; Turgut, P.; Bulut, H.; Isiker, Y. Investigation of the effects of pH, aging and scrap tire content on the dissolution behaviors of new scrap tire-concrete mixture structures. J. Clean. Prod. 2015, 93, 38–46. [Google Scholar] [CrossRef]
  14. Mohammed, B.S.; Adamu, M.; Shafiq, N. A review on the effect of crumb rubber on the properties of rubbercrete. Int. J. Civ. Eng. Technol. 2017, 8, 599–615. [Google Scholar]
  15. Al-Fakih, A.; Mohammed, B.S.; Wahab, M.M.A.; Liew, M.S.; Mugahed Amran, Y.H.; Alyousef, R.; Alabduljabbar, H. Characteristic compressive strength correlation of rubberized concrete interlocking masonry wall. Structures 2020, 26, 169–184. [Google Scholar] [CrossRef]
  16. Al-Fakih, A.; Wahab, M.M.A.; Mohammed, B.S.; Liew, M.S.; Wan Abdullah Zawawi, N.A.; As’ad, S. Experimental study on axial compressive behavior of rubberized interlocking masonry walls. J. Build. Eng. 2020, 29, 101107. [Google Scholar] [CrossRef]
  17. Chou, L.H.; Lu, C.-K.; Chang, J.-R.; Lee, M.T. Use of waste rubber as concrete additive. Waste Manag. Res. 2007, 25, 68–76. [Google Scholar] [CrossRef]
  18. Khed, V.C.; Mohammed, B.S.; Nuruddin, M.F. Effects of different crumb rubber sizes on the flowability and compressive strength of hybrid fibre reinforced ECC. In IOP Conference Series: Earth and Environmental Science; IOP Publishing: Bristol, UK, 2018. [Google Scholar] [CrossRef]
  19. Kanda, T.; Li, V.C. New micromechanics design theory for pseudostrain hardening cementitious composite. J. Eng. Mech. 1999, 125, 373–381. [Google Scholar] [CrossRef] [Green Version]
  20. Maalej, M.; Quek, S.T.; Ahmed, S.F.U.; Zhang, J.; Lin, V.W.J.; Leong, K.S. Review of potential structural applications of hybrid fiber Engineered Cementitious Composites. Constr. Build. Mater. 2012, 36, 216–227. [Google Scholar] [CrossRef]
  21. Phan, L. Fire Performance of High Strength Concrete: A Report of the State-of-the-Art; National Institute of Standards and Technology, Office of Applied Economics, Building and Fire Research Laboratory: Gaithersburg, MD, USA, 1996. [Google Scholar]
  22. Anderberg, Y. Spalling phenomena of HPC and OC. In NIST Workshop on Fire Performance of High Strength Concrete in Gaithersburg; U.S. Government Printing Office: North Capitol, WA, USA, 1997; pp. 69–73. [Google Scholar]
  23. Phan, L.T.; Lawson, J.R.; Davis, F.L. Effects of elevated temperature exposure on heating characteristics, spalling, and residual properties of high performance concrete. Mater. Struct. 2001, 34, 83–91. [Google Scholar] [CrossRef]
  24. Şahmaran, M.; Özbay, E.; Yücel, H.E.; Lachemi, M.; Li, V.C. Effect of Fly Ash and PVA Fiber on Microstructural Damage and Residual Properties of Engineered Cementitious Composites Exposed to High Temperatures. J. Mater. Civ. Eng. 2011, 23, 1735–1745. [Google Scholar] [CrossRef]
  25. Hernández-Olivares, F.; Barluenga, G. Fire performance of recycled rubber-filled high-strength concrete. Cem. Concr. Res. 2004, 34, 109–117. [Google Scholar] [CrossRef]
  26. ASTM C150/C150M-19a, Standard Specification for Portland Cement; ASTM International: West Conshohocken, PA, USA, 2019.
  27. ASTM C618-19, Standard Specification for Coal Fly Ash and Raw or Calcined Natural Pozzolan for Use in Concrete; ASTM International: West Conshohocken, PA, USA, 2019.
  28. ASTM C136/C136M-14, Standard Test Method for Sieve Analysis of Fine and Coarse Aggregates; ASTM International: West Conshohocken, PA, USA, 2014.
  29. Adamu, M.; Mohammed, B.S.; Shahir Liew, M. Mechanical properties and performance of high volume fly ash roller compacted concrete containing crumb rubber and nano silica. Constr. Build. Mater. 2018, 171, 521–538. [Google Scholar] [CrossRef]
  30. Montgomery, D.C. Design and Analysis of Experiments; John Wiley & Sons: Hoboken, NJ, USA, 2017. [Google Scholar]
  31. ASTM C109/C109M-16a, Standard Test Method for Compressive Strength of Hydraulic Cement Mortars (Using 2-in. or [50-mm] Cube Specimens); ASTM International: West Conshohocken, PA, USA, 2016.
  32. Rokugo, K. Recommendations for Design and Construction of High Performance Fiber Reinforced Cement Composites with Multiple Fine Cracks (HPFRCC); Japan Society of Civil Engineers, Gifu University: Gifu, Japan, 2008. [Google Scholar]
  33. ASTM C293/C293M-16, Standard Test Method for Flexural Strength of Concrete (Using Simple Beam with Center-Point Loading); ASTM International: West Conshohocken, PA, USA, 2016.
  34. ASTM C469/C469M-14, Standard Test Method for Static Modulus of Elasticity and Poisson’s Ratio of Concrete in Compression. ASTM International: West Conshohocken, PA, USA, 2016.
  35. ASTM C512/C512M-15, Standard Test Method for Creep of Concrete in Compression; ASTM International: West Conshohocken, PA, USA, 2015.
  36. ASTM C490/C490M-17, Standard Practice for Use of Apparatus for the Determination of Length Change of Hardened Cement Paste, Mortar, and Concrete; ASTM International: West Conshohocken, PA, USA, 2017.
  37. Mohammed, B.S.; Fang, O.C.; Anwar Hossain, K.M.; Lachemi, M. Mix proportioning of concrete containing paper mill residuals using response surface methodology. Constr. Build. Mater. 2012, 35, 63–68. [Google Scholar] [CrossRef]
Figure 1. Gradation curves for fine aggregates and crumb rubber.
Figure 1. Gradation curves for fine aggregates and crumb rubber.
Materials 14 03765 g001
Figure 2. Experimental testing setup for the (a) direct tensile test (dog-boned); (b) dog-boned-shaped dimensions (unit = mm); (c) three-point bending test; and (d) elastic modulus and Poisson’s ratio.
Figure 2. Experimental testing setup for the (a) direct tensile test (dog-boned); (b) dog-boned-shaped dimensions (unit = mm); (c) three-point bending test; and (d) elastic modulus and Poisson’s ratio.
Materials 14 03765 g002
Figure 3. (a) Demountable mechanical strain gauge point positions on creep specimen and (b) creep loading frame.
Figure 3. (a) Demountable mechanical strain gauge point positions on creep specimen and (b) creep loading frame.
Materials 14 03765 g003
Figure 4. (a) Creep strain and (b) creep coefficient of rubberized ECC containing nano-silica.
Figure 4. (a) Creep strain and (b) creep coefficient of rubberized ECC containing nano-silica.
Materials 14 03765 g004
Figure 5. The 3D response surface plots for 50% fly ash and 1% PVA fiber for (a) compressive strength, (b) flexural strength, (c) direct tensile strength, and (d) elastic modulus.
Figure 5. The 3D response surface plots for 50% fly ash and 1% PVA fiber for (a) compressive strength, (b) flexural strength, (c) direct tensile strength, and (d) elastic modulus.
Materials 14 03765 g005
Figure 6. The 3D response surface plots for 25% fly ash and 1% PVA fiber for (a) Poisson’s ratio and (b) drying shrinkage.
Figure 6. The 3D response surface plots for 25% fly ash and 1% PVA fiber for (a) Poisson’s ratio and (b) drying shrinkage.
Materials 14 03765 g006
Figure 7. The 3D response surface plot for 50% fly ash and 2% PVA fiber for (a) compressive strength, (b) flexural strength, (c) direct tensile strength, and (d) elastic modulus.
Figure 7. The 3D response surface plot for 50% fly ash and 2% PVA fiber for (a) compressive strength, (b) flexural strength, (c) direct tensile strength, and (d) elastic modulus.
Materials 14 03765 g007
Figure 8. The 3D response surface plot for 50% fly ash and 2% PVA fiber for (a) Poisson’s ratio and (b) drying shrinkage.
Figure 8. The 3D response surface plot for 50% fly ash and 2% PVA fiber for (a) Poisson’s ratio and (b) drying shrinkage.
Materials 14 03765 g008
Table 1. Chemical composition of cementitious materials.
Table 1. Chemical composition of cementitious materials.
ConfigurationCement (%)Fly Ash (%)
SiO2 (%)25.2158.35
Al2O3 (%)4.5920.96
Fe2O3 (%)2.994.9
CaO (%)62.859.79
MgO (%)1.701.99
Na2O (%)0.982.41
K2O (%)1.681.60
Specific gravity (g/cm3)3.152.38
Loss on ignition (%)2.21.25
Table 2. Nano-silica properties.
Table 2. Nano-silica properties.
ItemUnitQuality
Appearance-High-dispersive white powder
Hear reduction%≤3
Ignition loss%≤6
SiO2%≥99.8
Specific surface aream2/g100 ± 25
pH value-6.5–7.5
Surface densityg/mL≤0.15
Dispensability (CCl4)%≥80
Oil-absorbed valuemL/100 g≥250
Average particle sizenm10−25
Hydrophobicity-Strong
Table 3. PVA fiber physical properties.
Table 3. PVA fiber physical properties.
Fiber TypeSpecific Gravity (g/cm3)Elastic
Modulus
(GPa)
Length (mm)Diameter (μm)Aspect
Ratio
(L/d)
Tensile
Strength
(MPa)
PVA Fiber1.34112404621600
Table 4. Mixture constituents of each rubberized ECC model.
Table 4. Mixture constituents of each rubberized ECC model.
Mix Factors (%)Quantities (kg/m3)
w/cmCRFAPVANSOPCFAFine AggregateCRPVANSWater
M10.150010260.000.00210.600.005.850.0039.00
M20.152.55011130.00130.00205.341.895.852.6039.00
M30.1505002130.00130.00210.600.000.005.2039.00
M40.1552511195.0065.00200.073.755.852.6039.00
M50.152.52511195.0065.00205.341.895.852.6039.00
M60.150022260.000.00210.600.0011.705.2039.00
M70.152.5011260.000.00205.341.895.852.6039.00
M80.1505022130.00130.00210.600.0011.705.2039.00
M90.1555000130.00130.00200.073.750.000.0039.00
M100.1502511195.0065.00210.600.005.852.6039.00
M110.152.52511195.0065.00205.341.895.852.6039.00
M120.1505000130.00130.00210.600.000.000.0039.00
M130.152.52511195.0065.00205.341.895.852.6039.00
M140.150020260.000.00210.600.0011.700.0039.00
M150.152.52511195.0065.00205.341.895.852.6039.00
M160.1555020130.00130.00200.073.7511.700.0039.00
M170.152.52511195.0065.00205.341.895.852.6039.00
M180.152.52510195.0065.00205.341.895.850.0039.00
M190.1555022130.00130.00200.073.7511.705.2039.00
M200.152.52511195.0065.00205.341.895.852.6039.00
M210.1505020130.00130.00210.600.0011.700.0039.00
M220.152.52521195.0065.00205.341.8911.702.6039.00
M230.152.52512195.0065.00205.341.895.855.2039.00
M240.155000260.000.00200.073.750.000.0039.00
M250.1555002130.00130.00200.073.750.005.2039.00
M260.155002260.000.00200.073.750.005.2039.00
M270.150002260.000.00210.600.000.005.2039.00
M280.155022260.000.00200.073.7511.705.2039.00
M290.152.52501195.0065.00205.341.890.002.6039.00
M300.155020260.000.00200.073.7511.700.0039.00
w/cm: water-cementitious ratio, CR: crumb rubber, FA: fly ash, PVA: Polyvinyl-alcohol fiber, NS: nano silica, OPC: ordinary portland cement, FA: fly ash.
Table 5. Experimental design matrix and responses for rubberized ECC mixture.
Table 5. Experimental design matrix and responses for rubberized ECC mixture.
MixFactors (%)Responses
A: CRB: NSC: FAD: PVACS (MPa)ME (GPa) v DT (MPa)DS (µE)FS (MPa)
M1000187.1721.920.312.631103.708.95
M22.5150157.1129.650.262.821267.8010.75
M30250069.9127.140.343.131150.208.80
M45125148.1720.170.222.581323.909.50
M52.5125164.2925.260.262.701260.3010.75
M6020282.4424.750.243.401204.5010.20
M72.510165.0528.780.272.761284.4010.35
M80250283.4223.190.243.361203.709.95
M95050052.4421.670.212.911402.9010.25
M100125183.5729.570.252.731101.309.01
M112.5125165.2227.210.242.911281.3010.10
M120050083.8021.780.333.741124.808.89
M132.5125160.4522.900.242.821279.2010.05
M14000286.8126.350.292.591203.509.87
M152.5125163.0728.780.252.501283.3010.15
M165050244.9620.290.213.811401.3011.71
M172.5125168.4525.180.252.721280.1010.25
M182.5025167.6319.240.262.621281.309.95
M195250254.8620.110.213.811459.2010.05
M202.5125159.1025.230.252.891254.1010.25
M210050280.3623.320.242.991203.5010.20
M222.5125285.6818.110.232.971361.1012.20
M232.5225148.6921.210.252.971281.9011.40
M24500057.6619.210.212.811399.809.95
M255250048.9318.610.232.701403.3010.05
M26520051.1720.980.222.391402.4010.70
M27020069.5523.040.352.921250.308.90
M28520259.1019.240.273.191401.9011.35
M292.5125081.6322.370.243.121358.8011.10
M30500248.0917.930.293.551424.3010.990
A: crumb rubber, B: nano-silica, C: fly ash, D: PVA fiber, CS: compressive strength, ME: elastic modulus, v : Poisson’s ratio, DT: direct tensile strength, DS: drying shrinkage, and FS: flexural strength.
Table 6. ANOVA for the developed response models.
Table 6. ANOVA for the developed response models.
ResponseFactorsSquares SumD.F.Mean SquareF-Valuep-Value
Compressive strengthModel5108.1514364.8716.36<0.0001
A4169.6914169.69186.94<0.0001
B187.271187.278.400.0110
C131.611131.615.900.0282
D6.0416.040.270.6105
AB230.351230.3510.330.0058
AC8.8118.810.400.5391
AD9.8119.810.440.5173
BC59.18159.182.650.1241
BD294.851294.8513.220.0024
CD5.4815.480.250.6274
A20.005510.00550.000250.9877
B2156.031156.037.000.0184
C259.79159.792.680.1224
D2655.051655.0529.37<0.0001
Lack of Fit277.671027.772.440.0984
Elastic modulusModel272.601419.473.15<0.0001
A78.20178.2012.650.0029
B6.4716.471.050.3224
C3.4313.430.560.4676
D0.1810.180.0280.8686
AB5.2415.240.850.3718
AC0.01710.0170.00270.9592
AD3.6513.650.590.4544
BC1.5411.540.250.6250
BD2.9412.940.470.5013
CD2.6412.640.430.5234
A20.0009610.000960.000160.9902
B257.78157.789.350.0080
C249.70149.708.040.0125
D230.42130.424.920.0424
Lack of Fit72.46107.251.790.2707
Poisson’s ratioModel0.037140.00265916.31<0.0001
A0.01510.01500091.89<0.0001
B0.00004310.0000430.260.6155
C0.00204110.00204112.520.0030
D0.00274810.00274816.860.0009
AB0.00003910.0000390.240.6332
AC0.00029410.0002941.800.1995
AD0.01010.01000063.48<0.0001
BC0.00031110.0003111.910.1876
BD0.00086710.0008675.320.0358
CD0.00182010.00182011.170.0045
A20.00024810.0002481.520.2360
B20.00029410.0002941.810.1989
C20.00114110.0011417.000.0183
D20.00011710.0001170.720.4104
Lack of Fit0.002191100.0002194.310.1603
Direct tensile strengthModel3.53140.255.28<0.0001
A0.006810.00680.140.7116
B0.008110.00810.170.6857
C0.310.36.320.0238
D0.3610.367.440.0156
AB0.08910.0891.880.1910
AC0.003310.00330.0700.7949
AD0.9910.9920.860.0004
BC0.001510.00150.0310.8615
BD0.3110.316.600.0214
CD0.001610.00160.0340.8556
A20.01110.0110.230.6399
B20.01510.0150.320.5790
C20.01310.0130.280.6039
D20.3410.347.180.0171
Lack of Fit0.60100.0602.560.1551
Drying shrinkageModel279.401419,957.7061.52<0.0001
A208.501208.50642.82<0.0001
B768.451768.452.370.1446
C1195.3311195.333.680.0741
D1271.5711271.573.920.0664
AB107.751107.750.330.5730
AC2626.9612626.968.10.0123
AD0.1510.150.0004540.9833
BC138.081138.080.430.5240
BD56.32156.320.170.6828
CD2513.3112513.317.750.0139
A211,086.53111,086.5334.17<0.0001
B250.78150.780.160.6979
C23.2313.230.0099500.9219
D224,209.25124,209.2574.62<0.0001
Lack of Fit4084.3910408.442.610.1505
Flexural strengthModel272.601419.473.15<0.0001
A78.20178.2012.650.0029
B6.4716.471.050.3224
C3.4313.430.560.4676
D0.1810.180.0280.8686
AB5.2415.240.850.3718
AC0.01710.0170.0027000.9592
AD3.6513.650.590.4544
BC1.5411.540.250.6250
BD2.9412.940.470.5013
CD2.6412.640.430.5234
A20.00096410.0009640.0001560.9902
B257.78157.789.350.0080
C249.70149.708.040.0125
D230.42130.424.920.0424
Lack of Fit72.46107.251.790.2707
A: crumb rubber, B: nano-silica, C: fly ash, D: PVA fiber, A2, B2, C2, and D2: second order effect, AB, AC, AD, BC, BD, and CD: interaction effects, D.F: degree of freedom, F-value: Fisher-statistical test values, p-value: probability values.
Table 7. Model validation.
Table 7. Model validation.
ModelCompressive StrengthModulus ElasticityPoisson’s RatioDirect TensileDry ShrinkageFlexural Strength
R20.9390.9460.9380.9310.9830.944
Adj. R20.8810.9090.8810.8740.9670.898
Pred R20.6960.2840.5910.0860.8630.201
AP14.626.7315.939.1127.1110.44
S.D.4.722.490.0130.21818.010.461
μ65.9623.110.2552.971287.910.22
C.V.%7.1610.765.017.361.404.52
R2: correlation degree, Adj. R2: adjusted correlation degree, Pred R2: predicted correlation degree, AP: adequate precision, S.D.: standard deviation, μ: mean, and C.V.: coefficient of variation.
Table 8. Criteria for multi-objective optimization.
Table 8. Criteria for multi-objective optimization.
Factors and ResponsesNotationTargetLower LimitUpper Limit
Crumb rubber, %AIn range05
Nano-silica, %BIn range02
Fly ash, %CIn range050
PVA fiber, %DIn range02
Compressive strength, MPaCSTarget5050
Flexural strength, MPaFSMaximize8.812.2
Direct tensile strength, MPaDTMaximize2.3943.812
Elastic modulus, GPaMEMaximize17.9329.65
Poisson’s ratio v Minimize0.20890.347
Drying shrinkage, EDSMinimize1101.291459.24
Table 9. Optimized rubberized ECC mixtures.
Table 9. Optimized rubberized ECC mixtures.
CR, %NS, %FA, %PVA Fiber, %CS,
MPa
FS,
MPa
DT, MPaME,
GPa
v DS,
μE
Desirability, %
3.491.34542.141.24550.0010.6012.94122.0620.2401301.161.0
4.431.08543.511.07949.1010.0592.85325.9730.2181323.861.0
4.700.11847.031.97548.8011.3523.57419.910.2221427.211.0
Table 10. Validation of the experimental and predicted model.
Table 10. Validation of the experimental and predicted model.
CR, %NS, %FA, %PVA Fiber,
%
Results
&
Error
CS,
MPa
FS,
MPa
DT,
MPa
ME,
GPa
v DS,
μE
3.491.34542.141.245Predicted50.0010.6012.94122.0620.2401301.16
Experimental47.210.382.66520.380.2311226.96
Error, %5.602.089.387.623.755.70
4.4371.08543.511.079Predicted49.110.0592.85325.9730.2181323.86
Experimental45.769.622.74823.610.2001209.64
Error, %6.84.363.689.098.258.627
4.7030.11847.031.975Predicted48.811.3523.57419.910.2221427.21
Experimental46.2210.913.34119.370.2041349.77
Error, %5.283.896.522.718.105.43
Publisher’s Note: MDPI stays neutral with regard to jurisdictional claims in published maps and institutional affiliations.

Share and Cite

MDPI and ACS Style

Loganathan, R.; Mohammed, B.S. Properties of Rubberized Engineered Cementitious Composites Containing Nano-Silica. Materials 2021, 14, 3765. https://doi.org/10.3390/ma14133765

AMA Style

Loganathan R, Mohammed BS. Properties of Rubberized Engineered Cementitious Composites Containing Nano-Silica. Materials. 2021; 14(13):3765. https://doi.org/10.3390/ma14133765

Chicago/Turabian Style

Loganathan, Rubendran, and Bashar S. Mohammed. 2021. "Properties of Rubberized Engineered Cementitious Composites Containing Nano-Silica" Materials 14, no. 13: 3765. https://doi.org/10.3390/ma14133765

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.