Next Article in Journal
Siloxane Matrix Molecular Weight Influences the Properties of Nanocomposites Based on Metal Complexes and Dielectric Elastomer
Next Article in Special Issue
Characterizations and Antibacterial Efficacy of Chitosan Oligomers Synthesized by Microwave-Assisted Hydrogen Peroxide Oxidative Depolymerization Method for Infectious Wound Applications
Previous Article in Journal
Accelerated Bone Induction of Adult Rat Compact Bone Plate Scratched by Ultrasonic Scaler Using Acidic Electrolyzed Water
 
 
Font Type:
Arial Georgia Verdana
Font Size:
Aa Aa Aa
Line Spacing:
Column Width:
Background:
Article

CaCO3–Chitosan Composites Granules for Instant Hemostasis and Wound Healing

1
Department of Spine Surgery, Beijing JiShuiTan Hospital, 4th Medical College of Peking University, Xicheng District, Xinjiekou No. 31 East Street, Beijing 100035, China
2
Department of Orthopedics, The Third Affiliated Hospital of Guangzhou Medical University, 63 Duobao Road, Liwan District, Guangzhou 510150, China
3
Department of Spine Surgery, Zhejiang Provincial People’s Hospital, Hangzhou Medical College People’s Hospital, Hangzhou 310014, China
4
Department of Chemistry, Capital Normal University, Haidian District, Beijing 100035, China
*
Authors to whom correspondence should be addressed.
The authors contributed equally to this work.
Materials 2021, 14(12), 3350; https://doi.org/10.3390/ma14123350
Submission received: 5 March 2021 / Revised: 28 May 2021 / Accepted: 1 June 2021 / Published: 17 June 2021
(This article belongs to the Special Issue Novel Biomaterials for Soft and Hard Tissue Regeneration)

Abstract

:
Excessive bleeding induces a high risk of death and is a leading cause of deaths that result from traffic accidents and military conflict. In this paper, we developed a novel porous chitosan–CaCO3 (CS–CaCO3) composite material and investigated its hemostatic properties and wound healing performance. The CS–CaCO3 composites material was prepared via a wet-granulation method. Granulation increases the infiltrating ability of the CS–CaCO3 composites material. The improved water absorption ability was enhanced to 460% for the CS–CaCO3 composites material compared to the CaCO3 or chitosan with only one single component. The coagulation studies in vivo illustrated that the blood clotting time was greatly reduced from 31 s for CaCO3 to 16 s for the CS–CaCO3 composite material. According to the results of the wound healing experiments in rats, it was found that the CS–CaCO3 composite material can promote wound healing. The CS–CaCO3 composite material could accelerate wound healing to a rate of 9 days, compared with 12 days for the CaCO3. The hemostatic activity, biocompatibility, and low cost of CS–CaCO3 composite material make it a potential agent for effective hemostatic and wound healing materials.

1. Introduction

Hemorrhaging is a leading cause of deaths that result from traffic accidents and military conflict [1,2]. In hospitals, hemorrhage causes 15–25% of trauma deaths. A lot of hemostatic materials are used for hemorrhage controlling [3,4], which can be divided into inorganic materials [5,6,7] and organic polymer materials [8]. Inorganic materials include WoundStat, QuikClot, and Combat Gauze and polymer materials include Celox, Celox-D, HemCon, which are all commercially available products for hemostatic wound healing. However, the inorganic materials have many disadvantages, e.g., in the first generation of inorganic hemostatic materials, QuikClot caused high exothermic reactions and induced tissue empyrosis and other abnormal foreign-body reactions [9,10], and another inorganic material, WoundStat, induced thrombus in lungs and vessels [11,12]. Additionally, the poor adhesion of Combat Gauze made more blood loss [13]. Therefore, research is necessary to find more effective hemostatic agents.
Thrombin is an enzyme which can support earlier fibrin generation in the “waterfall reaction” of blood clotting. Calcium ions have the function to form thrombin and then activate the coagulation system. At the same time, intracellular Ca2+ can cause phosphatidyl serines to be exposed on platelet surfaces, and further help to assemble coagulation complexes and amplify the formation of thrombin [14,15]. Ca2+ can also stop bleeding by increasing clot rigidity. Similar to the benefit of Ca2+, CaCO3 also has good biocompatibility and potential for applications in medicine. In traditional Chinese medicine, cuttlebone, a kind of traditional hemostatic material that consists of CaCO3 is orally administered and can rapidly stop bleed [16,17,18,19,20,21]. Accordingly, developed hemostatic materials based on CaCO3 have been investigated for tissue repairing and rapid wound closure [22,23]
Chitosan is an inexpensive natural-origin polymer that has been widely used in clinics for its biodegradability, biocompatibility and antimicrobial activities [24,25]. Chitosan also has been widely investigated because of its hemostatic function [26,27,28,29,30]. The protonated amine groups of chitosan have a static interaction with the negative charge of red blood cells and platelets that induces formation of thrombus [31]. Chitosan also has good water absorption ability to facilitate hemostasis by blood coagulation factors and concentrating platelets [32,33,34]. Some commercially available materials have been developed based on chitosan as hemostatic agents such as Celox, TraumaStat, HemCon and so on. Chitosan-based materials demonstrated effective and safe properties for trauma application [35]. However, chitosan hemostatic materials cannot be used to treat wounds with heavy bleeding, because chitosan materials have no adhesion and may be washed away by blood, or chitosan materials may enter the blood vessels of the wound and cause thrombosis [36].
In this paper, we developed a novel CaCO3 and chitosan composite material used for hemorrhage control and wound healing due to their hemostatic properties and biocompatibility [37,38]. CaCO3 was mixed via wet-granulation method on chitosan by precipitation to improve the hemostatic activity of the composite material. The novel CS–CaCO3 composite material was characterized for its physicochemical properties. Due to the positive charge of the protonated amine group of chitosan, it can form a plug with the negative charge of erythrocytes cell membranes induced by electrostatic interaction, and then activate a coagulation cascade that brings a rapid and effective hemostasis (Scheme 1). In this manner, the CS–CaCO3 composite material exhibited excellent hemostatic and wound healing property on the injured site.

2. Experimental

2.1. Chemicals

Na2CO3 and CaCl2 were purchased from Sinopharm Chemical Reagent Ltd. (Beijing, China) and used to synthesis CaCO3 xerogel. Chitosan (Mw: 100,000–300,000 Da, from shrimp shells, deacetylated ratio ≥ 75%), were purchased from Integrated Scientific and Industrial Resource Platform (Beijing, China) and used for materials preparation and coatings. The MW of Chitosan was determined by the capillary viscometry method using an Ubbelohde viscometer Synthware Ltd. (Mainz, Germany)in the solution of 0.1 mol/L CH3COOH/0.2 mol/L NaCl at 25 °C, the viscosity average molecular weight (Mv) was calculated with vale of 367 kDa using the Mark−Houwink equation: [η] = KmMvα, where Km = 1.81 × 10−3, α = 0.93. The degree of deacetylation of CS was further determined by elemental analyses analysis on a Vario EL III CHN analyzer (Elementar Ltd. Stockport, UK) with the value of 77.8%. Fetal bovine serum was purchased from Invitrogen (Carlsbad, CA, USA). Other commercially available chemicals were used as received. High purity deionized water (18 MΩ) was used throughout this work, and all other chemicals used were of analytical grade.

2.2. Preparation of CS–CaCO3 Composites Materials

Calcium carbonate composites were synthesized by colloidal crystallization from supersaturated solution via wet-granulation method [39]. CaCl2 and Na2CO3 solution were rapidly mixed in equal volumes. Generally, 0.5 M Na2CO3 aqueous solution was rapidly poured into an equal volume of 0.5 M solution of CaCl2 at room temperature. Then, the precipitate was filtered off by suction filtration after intense agitation on a magnetic stirrer, thoroughly washed with pure water, and dried in vacuum. Chitosan was dissolved in 1% (w/v) aqueous acetic acid with fast stirring for 12 h to make 1% (w/v) chitosan solution, which was used as a dispersing phase. Then, the prepared CaCO3 powder was dispersed in 200 mL distilled water and poured into 200 mL chitosan solution. The CS–CaCO3 composite material were obtained after freeze-drying.

2.3. Characterization

The surface morphology of the CaCO3 and CS–CaCO3 was measured by scanning electron microscopy (SEM, SU8010, Hitachi, Hitachi, Japan). The CaCO3 and CS–CaCO3 composite material (5 µL) was dropped onto copper grid and dried in the air, then placed on aluminum stub and sputter coated with gold (10 mA for 90 s; JEOL JFC-1600) and imaged at 15 kV after complete air drying.
The X-ray diffraction (XRD) measurements were performed using a diffractometer (XD-3, MSAL, Purk Instrument Co. Ltd., Beijnig, China) with Cu (Ka) radiation at 36 kV and 20 mA. The characteristic XRD peaks of CaCO3, chitosan and CS–CaCO3 were compared to WH JCPDS (70−2064), International Center for Diffraction Data. (Beijing, China). The Fourier-transform infrared (FTIR) spectra were obtained using an infrared spectrometer (PerkinElmer, Waltham, MA, USA) from KBr pellets at wavelengths ranging from 4000 to 500 cm−1 at a resolution of 1 cm−1 with an average of 64 scans. The particle sizes were characterized by the DLS (Dynamic light scattering, Zetasizer Ultra, Marvin Co. Ltd., Marvin, UK)

2.4. Cell Viability Study

The cell viability of the CaCO3 and CS–CaCO3 was evaluated by Cell Counting Kit-8 (CCK-8) reduction (Kumamoto City, Japan). Assay with fibroblasts cell line (provided by National Center for Nanoscience and Technology, Beijing, China). Cells were cultured in medium containing 10% fetal bovine serum and 1% penicillin-streptomycin at 37 °C in 5% CO2-humidified air. Then 1 mL cell suspension was seeded into a 96-well plate (2 × 104 cells mL−1 per well) with medium containing CaCO3 and CS–CaCO3 with different concentration (0, 0.5, 1, 1.5, and 2 mg mL−1). 100 µL CCK-8 was added to each well after incubation for 24 h, and cells were cultured for another 4 h. Absorbance was recorded at 450 nm and cytotoxicity was determined as the percentage of viable cells relative to untreated control cells.

2.5. In Vitro Blood Plasma Coagulation Assay

The BALB/C rats (18–20 g) were purchased from the experimental center of the Zhejiang Provincial People’s Hospital, Hangzhou, China. This study was performed in strict accordance with the Guidelines for Care and Use of Laboratory Animals of Zhejiang Provincial People’s Hospital and approved by the Animal Ethics Committee of Zhejiang Provincial People’s Hospital. To explore the activation of CaCO3 and CS–CaCO3 material-induced blood plasma coagulation, the aPTT (activated partial thromboplastin time), PT (Prothrombin time) and TT (thrombin time)were determined in vitro coagulation assays, which were defined as the activated partial thromboplastin time, prothrombin time and thrombin time, respectively. This experiment was carried out with a full-automatic coagulation analyzer (Werfen Ltd., Birchwood, UK). The venous blood was drawn out from BALB/C rats and mixed with 3.8% (w/v) sodium citrate with the volume ratio 10:1. The platelet poor plasma (PPP) was obtained by whole blood centrifugation at 3000× g rpm/min for 20 min at 4 °C. PT and TT test was performed when 0.5 mL of citrated plasma and 5 mg/mL of simple were mixed and incubated at 37 °C for 5 min and measured by the automatic coagulation analyzer. For aPTT test, the mixture between 0.5 mL of citrated plasma and 5 mg/mL of simple was recalcified with 0.5 mL of 25 mM CaCl2 solution.

2.6. Blood Coagulation Time

Blood clotting potential of CaCO3 and CS–CaCO3 composite material systems was examined according to the reference [26]. 100 mg of CaCO3 and CS–CaCO3 composite material were put into the 48-well plate. Then 50 µL of 25 mM CaCl2 solution was added to 250 µL calcified blood, 300 µL of the rat blood solution prepared was added into the wells. The wells were then washed using 0.9% NaCl solution to remove the unclotted blood. The blood clotting time was defined as the time at which the formation was uniform and there were stable clots in the wells.

2.7. Adherence of RBC (Red blood cell) and Platelet on CaCO3 and CS–CaCO3 Composite Material

The BALB/C rat blood with citrate was added with 1 mg of CaCO3 or the CS–CaCO3 composite material and then incubated at 37 °C for 30 min. The precipitates were filtered and washed 3 times with PBS (phosphate buffered saline), and then 2.5% glutaraldehyde solution was added to the precipitates and kept at room temperature. After 2.5 h, the precipitates were washed with PBS and dehydrated in ethanol solution with different concentration (20%, 40%, 60%, 80% and 100%), and then dried in the air. The BALB/C rat blood was added with citrate and then the Platelet Rich Plasma (PRP) was seperated by centrifuging at 2000 rpm/min for 20 min. The upper PRP layer was taken out by pipette and added into the cuvet containing CaCO3 or CS–CaCO3, and then they were incubated at 37 °C for 30 min. The precipitation was collected and treated in the same way with RBCs. The adhesion and morphology of the platelet CaCO3 and CS–CaCO3 composite material were observed by SEM after being coated with gold.

2.8. Water Absorption Efficiency In Vitro

CaCO3 and CS–CaCO3 composite materials were weighed as the same mass and immersed in the PBS buffer with pH 7.4 at 37 °C overnight. The CaCO3 and CS–CaCO3 composite materials were taken out from PBS buffer at same time intervals, then the water was wiped up with filter paper gently and immediately. The water absorption ratio (A) was calculated by:
A = M W M d M d × 100 %
In the above equation, A is swelling ratio, Mw is the wet weight of the materials and Md is the dry weight of the materials.

2.9. Hemolysis Assay

The BALB/C rat blood was transferred into 3.8% sodium citrated solution. The collected blood was centrifuged at 2000× g rpm/min to separate the RBCs. Then one milliliter of concentrated RBCs was diluted with saline solution. The hemolytic activity of the CaCO3 and CS–CaCO3 with different concentrations (0.5, 1.0, 2.0, 3.0, and 5.0 mg/mL) were examined. The samples in 0.1% Triton-X (100 µL) were used as positive control and the samples in saline (100 µL) were used as negative control. Diluted 2% w/v RBCs (500 µL) was added and incubated at 37 °C for 1 h. Then the samples were centrifuged (3500× g rpm; 10 min) to obtain the supernatant. The collected supernatant was determined by spectrophotometry as having an absorbance value of 540 nm using a well plate reader. Percent hemolysis (%) was calculated following the equation as below:
Hemolysis   % = A sample A PBS A water A PBS × 100 %
In this expression, Asample, APBS, Awater represent the absorbance value of test samples, positive (water), and negative (PBS) controls

2.10. In Vivo Wound Healing

The rats used to assess hemostatic performance were divided into five groups, each group contains three rats. Every group of rats took normal feed and water without restriction. The rats were anesthetized by intramuscular injection with 1% pentobarbital sodium. The dorsal area of the rats was depilated and cleaned with alcohol. A wound of 1 cm2 was produced by excising the skin of the rat. The rats with bare wounds were used as a negative control, and the other rats with the wounds were covered with CaCO3 and CS–CaCO3 to measure the wound healing property of the novel material. After covering the materials, the rats were returned individually in cages under normal room temperature. The covering materials were changed at day 1, 2, and 3, and the wound area was measured with a ruler and photographs were taken. The rats were recovered in 2 weeks to be used for evaluating wound-healing properties of the CaCO3, and CS–CaCO3.
The percent reduction in wound size was calculated as the formula as below:
reduction % = W 0 W t W 0 × 100 %
In this expression, W0 and Wt represent the wounds size on the 1st day and the 7th day, respectively.
After day 14, the skin wound tissue of the rat was excised and fixed with 10% formalin to be stained with a hematoxylin−eosin. Histological analysis was measured by H&E and Masson’s trichrome.

3. Result and Discussion

3.1. Characterization of the Prepared of CaCO3 and CS–CaCO3 Composites Materials

CaCO3 and CS–CaCO3 were synthesized by colloidal crystallization from supersaturated solution and obtained after freeze-drying. SEM images of the prepared CaCO3 showed spherical-shaped morphology and with particle size of 3 µm (Figure 1a). In Figure 1b,c, the CS–CaCO3 displays spherical-shaped particles and an increased surface roughness, respectively, which was attributed to surface complexation resulting from the complexation of CaCO3 and chitosan. In Figure 2, the DLS (Dynamic light scattering) results exhibit the particle radius of CaCO3 and CS–CaCO3 of about 600 nm, and the polydispersity index of CaCO3 and CS–CaCO3 are 1.34 and 1.22, respectively; these results are in accordance with the SEM results and indicate remarkable monodispersion of the synthesized CaCO3 and CS–CaCO3.
Presence of CaCO3 and CS–CaCO3 in the novel material was further illustrated by FTIR. FTIR data of the developed CS–CaCO3 composite material (Figure 3a) showed the characteristics peaks of CaCO3 at 713, 877, and 1427 cm−1 (−CO3 stretching) and characteristics peaks of Chitosan at 1070 (−C−O stretch), 1425, 1566 (−N−H stretch) and 2920 cm−1 (−C−H stretch), which indicated the presence of CaCO3 in the CS–CaCO3 composite materials.
The CaCO3, chitosan, and CS–CaCO3 were further characterized by XRD analysis. The XRD peaks obtained for the CaCO3 particles matched with the XRD peaks of CaCO3 that corresponded to calcite (The Inorganic Crystal Structure Database (ICSD) no. 158257) [28]. It is evident that native Chitosan had characteristic broad peaks at 21.08, which are typical of a chitosan structure. In the XRD spectra of CS–CaCO3, the characteristic peak of CaCO3 at 2θ of 23.44°, 29.76°, 36.34°, 39.8°, 43.5°, 47.84°, 48.94° was observed (Figure 3b). This further confirmed the presence of CaCO3 in the composite materials. The crystallinity of CaCO3 was higher than CS–CaCO3. There was almost no difference in crystallinity between CaCO3 and CS–CaCO3. The result indicated that complexation did not disrupt the ordered structure of the crystalline regions in CaCO3. The CS–CaCO3 was successfully fabricated by complexation between amino groups and Ca2+ [40].

3.2. Fluid Sorption Capability

CaCO3 and CS–CaCO3 were studied for water absorption for 24 h at room temperature. Figure 4 shows the water absorption ratio of CaCO3 was 124%, however, the water absorption ratio for chitosan and CS–CaCO3 can reach 345% and 459%, which is much higher than that of CaCO3. The water absorption rate of CaCO3 was low, which can be attributed to only a small surface area of inorganic compound CaCO3. The water absorption amount increased with the porous structure formation on the material surface. The water absorption of pure can get to 350 % because of the capillary action. However, the equilibrium water absorption amount of CS–CaCO3 was the highest, which may be contributed to by the CaCO3 particles having high surface area and the combination of the chitosan capillary action.

3.3. Cytotoxicity Tests of the CS–CaCO3

A good hemostatic agent must have high biocompatibility and low cytotoxicity. Therefore, fibroblast cells were treated with various concentrations of CaCO3 and CS–CaCO3 to measure the cytotoxicity of the novel hemostatic material. Cell viability was achieved using CCK-8 assay and live/dead viability assay. Figure 5 shows that both CaCO3 and CS–CaCO3 could significantly promote cell viability, which demonstrates that CaCO3 and CS–CaCO3 have high biocompatibility and low cytotoxicity and have the potential application for hemostatic materials.

3.4. Blood Clotting Activity

Blood clotting time measurement can be used to reflect the hemostatic potential of a novel material. As shown in Figure 6a, compared with control and CaCO3, blood clotting time decreased greatly for the sample added with the CS–CaCO3. The results of blood clotting time indicated that CS–CaCO3 might have better hemostatic performance. Hemostasis can prevent a large amount of blood loss after vascular injury. It depends on a complex process including platelets, other cells and the activation of specific blood proteins known as coagulation factors.
In vitro activated partial thromboplastin time (aPTT), thrombin time (TT) and prothrombin time (PT) were measured to estimate the hemostasis. Figure 6 shows the APPTs, TTs and PTs of samples results. Compared with the control, the aPTT of CS–CaCO3 at the concentration of 0.5 mg/mL and 1.0 mg/mL kept the same but the aPTT of CaCO3 dropped from 54 to 50 s. For both of the concentrations, the aPTT of CS–CaCO3 is shorter than CaCO3 (Figure 6b). Figure 6c,d shows that the TTs and PTs of samples follow a similar trend, and no significant dosage-dependent relationship was observed for both CaCO3 and CS–CaCO3. The results illustrate that the CS–CaCO3 could not only decrease the time of thromboplastin formation, but also accelerate the activation of the intrinsic coagulation system. The addition of CaCO3 and CS–CaCO3 accelerate the coagulation system.

3.5. Hemolytic Activity

A hemolysis assay was used to determine the toxicity of CS–CaCO3 on RBCs. A total of 2.0 mL of isolated RBCs was mixed with CaCO3 and CS–CaCO3 with different concentrations in PBS at a range of 0.5 to 2.0 mg mL−1 and incubated at room temperature for 1 h. Additionally, positive and negative control samples were prepared by adding 2.0 mL of water and PBS respectively to RBCs. At every 30 min, precipitated cells and particles were resuspended by gentle shaking. The photographs showing precipitated RBCs at the end of the hemolysis experiment are given in Figure 7a. The red color of the released hemoglobin from damaged cells is clearly observable for the positive control. For CaCO3 and CS–CaCO3, the supernatants are almost colorless at all concentrations, which illustrates the CaCO3 and CS–CaCO3 can almost completely prevent the hemolytic activity.
Hemolytic activity of the CS–CaCO3 was determined by measuring the absorption peak of hemoglobin at 540 nm, which was released to the solution from the hemolyzed cells. Hemolysis results for both CaCO3 and CS–CaCO3 are given in Figure 7. CaCO3 showed the higher hemolytic activity than CS–CaCO3, which was observed for all the experiment concentrations. On the other hand, the hemolytic activity of CaCO3 kept the value between 1.4~1.9%; however, the hemolytic activity of CS–CaCO3 increased with the concentration. The photographs showing precipitated RBCs at the end of the hemolysis experiment are given in Figure 7a. The red color of the released hemoglobin from damaged cells is clearly observable for CS–CaCO3. For CS–CaCO3 the supernatants are almost colorless at all concentrations. Therefore, the percentage of hemolysis of the CaCO3 and CS–CaCO3 was found to be less than 5%, which is an allowable limit for biomaterials, which exhibited that CaCO3 and CS–CaCO3 composite materials were hemocompatible.

3.6. Platelet Adhesion

The platelet adhesion property of the CaCO3 and CS–CaCO3 was determined by agitation of the samples, and then SEM was conducted to observe the capture of adherent platelets of prepared samples (Figure 8). The SEM images show the platelets adhered to the CS–CaCO3 and illustrate the morphology of the adhered platelets being exposed to the materials after 30 min. The surfaces of CaCO3 and CS–CaCO3 were both covered with a lot of adhered platelets. It can be estimated that the platelet aggregation was stimulated by CaCO3 and CS–CaCO3. The result illustrates that CaCO3 and CS–CaCO3 promoted the aggregation and activation of platelets. At the same time, RBCs were observed with good dispersity and biconcave shape. With the addition of CaCO3 and CS–CaCO3, RBCs joined together with roughly linear chains, which demonstrates CaCO3 and CS–CaCO3 can cause RBC aggregation.

3.7. Wound Healing

Last, the prepared CaCO3 and CS–CaCO3 was conducted in vivo to prove the enhanced wound healing ability. We examined the wound-healing properties of CaCO3 and CS–CaCO3 in vivo by treating a small cut (1 cm × 1 cm) with CaCO3 or CS–CaCO3 for 3, 5, 7, and 9 d, and bare wounds were used as the control (Figure 9). The extent of wound healing was evaluated macroscopically. Wounds were almost completely healed after 10 d which were treated with CS–CaCO3. Compared to the control group, the CaCO3 and CS–CaCO3 treatment group both exhibited a more rapid recovering of wound size, especially in the first 7 d (Figure 9a).
Furthermore, qualitative histomorphologies stained by hematoxylin and eosin sections were studied. The wound healing was comprised of three stages: inflammation, new tissue formation, and remodeling healing. Histological analysis showed the extent of collagen deposition of the wound treated with CaCO3 and CS–CaCO3, which was confirmed by H&E-stained images (Figure 10). New blood vessels and glandular cavity was shown in wounds treated with CaCO3 and CS–CaCO3, which illustrated cell proliferation and new tissue formation in the wound. The epithelial tissue of the CS–CaCO3 wound after 10 d revealed the best wound healing properties compared to those treated with CaCO3 and without treatment. The collagen content of the wound area was studied by Masson’s trichrome staining. The density of the collagen fiber in the wounds was increased upon treatment with CaCO3 and CS–CaCO3 as compared to the control group (Figure 10). These results indicate that CS–CaCO3 are not only procoagulant but also have wound healing capacity.

4. Conclusions

In conclusion, we developed a CS–CaCO3 composites material which can be used for hemorrhage control and wound healing. Compared with single CaCO3, the CS–CaCO3 composite material showed shorter bleeding time and better wound-healing performance. Otherwise, the CS–CaCO3 composite material also exhibited a stronger fluid absorbance property of concentrated RBCs, blood platelets, and clotting factors. The CS–CaCO3 composite material activated the intrinsic coagulation cascade, showing better hemorrhage control, biocompatibility and wound healing property than the CaCO3 granules. Our results illustrated that the CS–CaCO3 composite material can be used to prevent massive blood loss and that it is an effective hemostatic agent.

Author Contributions

Conceptualization, D.H. and X.H. (Xiaonan Huang); methodology, W.H.; software, Q.W.; validation, Y.Z. and B.L.; formal analysis, Y.Z.; investigation, B.L.; resources, Y.Z. and Y.L.; data curation, J.Z.; writing—original draft preparation, W.H. and D.H.; writing—review and editing, W.H.; visualization, X.H. (Xiaodong Huang); supervision, B.L.; project administration, Y.L. and D.H.; funding acquisition, W.H. All authors have read and agreed to the published version of the manuscript.

Funding

This study was funded by Capital’s Funds for Health Improvement and Research (2020-2-2072), Beijing Natural Science Foundation (L202005), Beijing Jishuitan Hospital “Nova Program” (#XKXX201808), and Beijing Hospital Authority Youth Program (#QML20190403).

Institutional Review Board Statement

The study was conducted according to the guidelines of the Declaration of Helsinki, and approved by the Animal Ethical and Welfare Committee of Zhejiang Province People’s Hospital (protocol code A20210005 and 22 March 2021).

Informed Consent Statement

Informed consent was obtained from all subjects involved in the study.

Data Availability Statement

The data reported in this article are available on request from the corresponding author.

Conflicts of Interest

The authors declare no conflict of interest.

References

  1. Alam, H.B.; Burris, D.; DaCorta, J.A.; Rhee, P. Hemorrhage Control in the Battlefield: Role of New Hemostatic Agents. Mil. Med. 2005, 170, 63–69. [Google Scholar] [CrossRef] [PubMed] [Green Version]
  2. Abassi, Z.A.; Okun-Gurevich, M.; Abu Salah, N.; Awad, H.; Mandel, Y.; Campino, G.; Mahajna, A.; Feuerstein, G.Z.; Fitzpatrick, M.; Hoffman, A.; et al. Potential Early Predictors for Outcomes of Experimental Hemorrhagic Shock Induced by Un-controlled Internal Bleeding in Rats. PLoS ONE 2013, 8, e80862. [Google Scholar] [CrossRef] [PubMed]
  3. Gaston, E.; Fraser, J.F.; Xu, Z.P.; Ta, H.T. Nano- and micro-materials in the treatment of internal bleeding and uncontrolled hemorrhage. Nanomed. Nanotechnol. Biol. Med. 2018, 14, 507–519. [Google Scholar] [CrossRef] [Green Version]
  4. Pusateri, A.E.; Holcomb, J.B.; Kheirabadi, B.S.; Alam, H.B.; Wade, C.E.; Ryan, K.L. Making Sense of the Preclinical Literature on Advanced Hemostatic Products. J. Trauma Inj. Infect. Crit. Care 2006, 60, 674–682. [Google Scholar] [CrossRef] [PubMed]
  5. Li, H.; Wang, L.; Alwaal, A.; Lee, Y.-C.; Reed-Maldonado, A.; Spangler, T.A.; Banie, L.; O’Hara, R.B.; Lin, G. Comparison of Topical Hemostatic Agents in a Swine Model of Extremity Arterial Hemorrhage: BloodSTOP iX Battle Matrix vs. QuikClot Combat Gauze. Int. J. Mol. Sci. 2016, 17, 545. [Google Scholar] [CrossRef] [PubMed] [Green Version]
  6. Otrocka-Domagała, I.; Jastrzębski, P.; Adamiak, Z.; Paździor-Czapula, K.; Gesek, M.; Mikiewicz, M.; Rotkiewicz, T. Safety of the long-term application of QuikClot Combat Gauze, ChitoGauze PRO and Celox Gauze in a femoral artery injury model in swine—A preliminary study. Pol. J. Vet. Sci. 2016, 19, 337–343. [Google Scholar] [CrossRef] [PubMed] [Green Version]
  7. Littlejohn, L.F.; Devlin, J.J.; Kircher, S.S.; Lueken, R.; Melia, M.R.; Johnson, A.S. Comparison of Celox-A, ChitoFlex, WoundStat, and Combat Gauze Hemostatic Agents Versus Standard Gauze Dressing in Control of Hemorrhage in a Swine Model of Penetrating Trauma. Acad. Emerg. Med. 2011, 18, 340–350. [Google Scholar] [CrossRef]
  8. Kheirabadi, B.S.; Scherer, M.R.; Estep, J.S.; Dubick, M.A.; Holcomb, J.B. Determination of Efficacy of New Hemostatic Dressings in a Model of Extremity Arterial Hemorrhage in Swine. J. Trauma Inj. Infect. Crit. Care 2009, 67, 450–460. [Google Scholar] [CrossRef] [PubMed]
  9. Lee, M.-Y.; Bae, O.-N.; Chung, S.-M.; Kang, K.-T.; Lee, J.-Y.; Chung, J.-H. Enhancement of Platelet Aggregation and Thrombus Formation by Arsenic in Drinking Water: A Contributing Factor to Cardiovascular Disease. Toxicol. Appl. Pharmacol. 2002, 179, 83–88. [Google Scholar] [CrossRef]
  10. Singh, S.K.; Singh, M.K.; Nayak, M.K.; Kumari, S.; Shrivastava, S.; Grácio, J.; Dash, D. Thrombus Inducing Property of Atomically Thin Graphene Oxide Sheets. ACS Nano 2011, 5, 4987–4996. [Google Scholar] [CrossRef]
  11. Arnaud, F.; Tomori, T.; Carr, W.; McKeague, A.; Teranishi, K.; Prusaczyk, K.; McCarron, R. Exothermic reaction in zeolite hemostatic dressings: QuikClot ACS and ACS+(R). Ann. Biomed. Eng. 2008, 36, 1708–1713. [Google Scholar] [CrossRef]
  12. Zhou, H.; Wang, C.; Niu, H.; Duan, B.; Ma, X.; Hong, H.; Yuan, Y.; Liu, C. A Novel Droplet-Fabricated Mesoporous Silica-Based Nanohybrid Granules for Hemorrhage Control. J. Biomed. Nanotechnol. 2018, 14, 649–661. [Google Scholar] [CrossRef]
  13. De Castro, G.P.; Dowling, M.B.; Kilbourne, M.; Keledjian, K.; Driscoll, I.R.; Raghavan, S.R.; Hess, J.R.; Scalea, T.M.; Bochicchio, G.V. Determination of efficacy of novel modified chitosan sponge dressing in a lethal arterial injury model in swine. J. Trauma: Inj. Infect. Crit. Care 2012, 72, 899–907. [Google Scholar] [CrossRef] [Green Version]
  14. Jang, J.K.; Lee, O.S.; Kang, T.J.; Lim, S.C. Wound healing effect of cuttlebone extract in burn injury of rat. Food Sci. Biotechnol. 2013, 22, 99–105. [Google Scholar] [CrossRef]
  15. Lv, L.; Tang, F.; Lan, G. Preparation and characterization of a chitin/platelet-poor plasma composite as a hemostatic material. RSC Adv. 2016, 6, 95358–95368. [Google Scholar] [CrossRef]
  16. Garcia, J.G.N.; Patterson, C.; Bahler, C.; Aschner, J.; Hart, C.M.; English, D. Thrombin receptor activating peptides induce Ca2+ mobilization, barrier dysfunction, prostaglandin synthesis, and platelet-derived growth-factor messenger-rna expression in cultured endothelium. J. Cell. Physiol. 1993, 156, 541–549. [Google Scholar] [CrossRef]
  17. Cavallini, L.; Alexandre, A. Ca2+ efflux from platelets. Control by protein kinase C and the filling state of the intracellular Ca2+ stores. JBIC J. Biol. Inorg. Chem. 1994, 222, 693–702. [Google Scholar] [CrossRef]
  18. Franke, B.; Akkerman, J.N.; Bos, J.L. Rapid Ca2+-mediated activation of Rap1 in human platelets. EMBO J. 1997, 16, 252–259. [Google Scholar] [CrossRef] [Green Version]
  19. Alonso, M.T.; Alvarez, J.; Montero, M.; Sanchez, A.; García-Sancho, J. Agonist-induced Ca2+ influx into human platelets is secondary to the emptying of intracellular Ca2+ stores. Biochem. J. 1991, 280, 783–789. [Google Scholar] [CrossRef] [Green Version]
  20. Varga-Szabo, D.; Braun, A.; Nieswandt, B. Calcium signaling in platelets. J. Thromb. Haemost. 2009, 7, 1057–1066. [Google Scholar] [CrossRef]
  21. Kahn, M.L.; Zheng, Y.-W.; Huang, W.; Bigornia, V.; Zeng, D.; Moff, S.L.; Jr, R.V.F.; Tam-Amersdorfer, C.; Coughlin, S.R. A dual thrombin receptor system for platelet activation. Nat. Cell Biol. 1998, 394, 690–694. [Google Scholar] [CrossRef] [PubMed]
  22. Shamshina, J.L.; Gurau, G.; Block, L.E.; Hansen, L.K.; Dingee, C.; Walters, A.; Rogers, R.D. Chitin–calcium alginate composite fibers for wound care dressings spun from ionic liquid solution. J. Mater. Chem. B 2014, 2, 3924–3936. [Google Scholar] [CrossRef]
  23. Francesko, A.; Tzanov, T. Chitin, Chitosan and Derivatives for Wound Healing and Tissue Engineering. In Biofunctionalization of Polymers and Their Applications; Nyanhongo, G.S., Steiner, W., Gubitz, G.M., Eds.; Springer: Berlin/Heidelberg, Germany, 2011; Volume 125, pp. 1–27. [Google Scholar]
  24. Pillai, C.; Paul, W.; Sharma, C.P. Chitin and chitosan polymers: Chemistry, solubility and fiber formation. Prog. Polym. Sci. 2009, 34, 641–678. [Google Scholar] [CrossRef]
  25. Agboh, O.C.; Qin, Y. Chitin and chitosan fibers. Polym. Adv. Technol. 1997, 8, 355–365. [Google Scholar] [CrossRef]
  26. Ong, S.-Y.; Wu, J.; Moochhala, S.M.; Tan, M.-H.; Lu, J. Development of a chitosan-based wound dressing with improved hemostatic and antimicrobial properties. Biomaterials 2008, 29, 4323–4332. [Google Scholar] [CrossRef]
  27. Rao, S.B.; Sharma, C.P. Use of chitosan as a biomaterial: Studies on its safety and hemostatic potential. J. Biomed. Mater. Res. 1997, 34, 21–28. [Google Scholar] [CrossRef]
  28. Kim, I.-Y.; Seo, S.-J.; Moon, H.-S.; Yoo, M.-K.; Park, I.-Y.; Kim, B.-C.; Cho, C.-S. Chitosan and its derivatives for tissue engineering applications. Biotechnol. Adv. 2008, 26, 1–21. [Google Scholar] [CrossRef] [PubMed]
  29. Yang, J.; Tian, F.; Wang, Z.; Wang, Q.; Zeng, Y.-J.; Chen, S.-Q. Effect of chitosan molecular weight and deacetylation degree on hemostasis. J. Biomed. Mater. Res. Part B Appl. Biomater. 2007, 84, 131–137. [Google Scholar] [CrossRef]
  30. Aam, B.B.; Heggset, E.B.; Norberg, A.L.; Sørlie, M.; Vårum, K.M.; Eijsink, V.G.H. Production of Chitooligosaccharides and Their Potential Applications in Medicine. Mar. Drugs 2010, 8, 1482–1517. [Google Scholar] [CrossRef] [Green Version]
  31. Klokkevold, P.R.; Fukayama, H.; Sung, E.C.; Bertolami, C.N. The effect of chitosan (poly-N-acetyl glucosamine) on lingual hemostasis in heparinized rabbits. J. Oral Maxillofac. Surg. 1999, 57, 49–52. [Google Scholar] [CrossRef]
  32. Chae, S.Y.; Jang, M.-K.; Nah, J.-W. Influence of molecular weight on oral absorption of water soluble chitosans. J. Control. Release 2005, 102, 383–394. [Google Scholar] [CrossRef]
  33. Wang, Y.N.; Fu, Y.M.; Li, J.; Mu, Y.Z.; Zhang, X.; Zhang, K.C.; Liang, M.Q.; Feng, C.; Chen, X.G. Multifunctional chi-tosan/dopamine/diatom-biosilica composite beads for rapid blood coagulation. Carbohydr. Polym. 2018, 200, 6–14. [Google Scholar] [CrossRef]
  34. Chung, Y.-C.; Su, Y.-P.; Chen, C.-C.; Jia, G.; Wang, H.-L.; Wu, J.C.G.; Lin, J.-G. Relationship between antibacterial activity of chitosan and surface characteristics of cell wall. Acta Pharmacol. Sin. 2004, 25, 932–936. [Google Scholar]
  35. Agnihotri, S.A.; Mallikarjuna, N.N.; Aminabhavi, T.M. Recent advances on chitosan-based micro- and nanoparticles in drug delivery. J. Control. Release 2004, 100, 5–28. [Google Scholar] [CrossRef] [PubMed]
  36. Reinthaler, M.; Braune, S.; Lendlein, A.; Landmesser, U.; Jung, F. Platelets and coronary artery disease: Interactions with the blood vessel wall and cardiovascular devices. Biointerphases 2016, 11, 029702. [Google Scholar] [CrossRef]
  37. Peng, C.Y.; Zhao, Q.H.; Gao, C.Y. Sustained delivery of doxorubicin by porous CaCO3 and chitosan/alginate multi-layers-coated CaCO3 microparticles. Colloid Surf. A Physicochem. Eng. Asp. 2010, 353, 132–139. [Google Scholar] [CrossRef]
  38. Wang, J.; Chen, J.-S.; Zong, J.-Y.; Zhao, D.; Li, F.; Zhuo, R.-X.; Cheng, S.-X. Calcium Carbonate/Carboxymethyl Chitosan Hybrid Microspheres and Nanospheres for Drug Delivery. J. Phys. Chem. C 2010, 114, 18940–18945. [Google Scholar] [CrossRef]
  39. Volodkin, D.V.; Larionova, N.I.; Sukhorukov, G.B. Protein Encapsulation via Porous CaCO3 Microparticles Templating. Biomacromolecules 2004, 5, 1962–1972. [Google Scholar] [CrossRef]
  40. Zhou, Y.; Li, H.; Liu, J.; Xu, Y.; Wang, Y.; Ren, H.; Li, X. Acetate chitosan with CaCO3 doping form tough hydrogel for hemostasis and wound healing. Polym. Adv. Technol. 2019, 30, 143–152. [Google Scholar] [CrossRef] [Green Version]
Scheme 1. Schematic representation of hemostatic material CS–CaCO3.
Scheme 1. Schematic representation of hemostatic material CS–CaCO3.
Materials 14 03350 sch001
Figure 1. SEM images of (a) CaCO3 and (b) chitosan and (c) CS–CaCO3.
Figure 1. SEM images of (a) CaCO3 and (b) chitosan and (c) CS–CaCO3.
Materials 14 03350 g001
Figure 2. DLS results of (a) CaCO3 and (b) CS–CaCO3.
Figure 2. DLS results of (a) CaCO3 and (b) CS–CaCO3.
Materials 14 03350 g002
Figure 3. (a) XRD pattern of CaCO3, CS and CS–CaCO3; and (b) FTIR spectra of CaCO3, CS and CS–CaCO3.
Figure 3. (a) XRD pattern of CaCO3, CS and CS–CaCO3; and (b) FTIR spectra of CaCO3, CS and CS–CaCO3.
Materials 14 03350 g003
Figure 4. Water absorbability of CaCO3 and CS–CaCO3.
Figure 4. Water absorbability of CaCO3 and CS–CaCO3.
Materials 14 03350 g004
Figure 5. Viability of fibroblast cells after 12 h exposure to various materials and negative control (TCPS). Data were obtained using CCK-8 assay.
Figure 5. Viability of fibroblast cells after 12 h exposure to various materials and negative control (TCPS). Data were obtained using CCK-8 assay.
Materials 14 03350 g005
Figure 6. Blood coagulation test in vitro. (a) Blood clotting time, (b) aPTT, (c) TT and (d) PT measurement of CaCO3 and CS–CaCO3.
Figure 6. Blood coagulation test in vitro. (a) Blood clotting time, (b) aPTT, (c) TT and (d) PT measurement of CaCO3 and CS–CaCO3.
Materials 14 03350 g006
Figure 7. (a) Images of RBCs incubated with CaCO3 and CS–CaCO3 at 37 °C for 1 h; (b) Hemolysis assay for CaCO3 and CS–CaCO3.
Figure 7. (a) Images of RBCs incubated with CaCO3 and CS–CaCO3 at 37 °C for 1 h; (b) Hemolysis assay for CaCO3 and CS–CaCO3.
Materials 14 03350 g007
Figure 8. SEM images of erythrocyte agglutination and adhesion on the surfaces of (A) CaCO3-chitason and (B) CaCO3.
Figure 8. SEM images of erythrocyte agglutination and adhesion on the surfaces of (A) CaCO3-chitason and (B) CaCO3.
Materials 14 03350 g008
Figure 9. (a) The wound area dependence of time (d) treated by CaCO3, CaCO3-chitason and without treating as the control; (b) Images of wounds left untreated or treated with CaCO3 and CaCO3-chitason immediately following surgery (day 0), and after 3, 5, 7, or 10 d. Scale bars, 0.25 cm.
Figure 9. (a) The wound area dependence of time (d) treated by CaCO3, CaCO3-chitason and without treating as the control; (b) Images of wounds left untreated or treated with CaCO3 and CaCO3-chitason immediately following surgery (day 0), and after 3, 5, 7, or 10 d. Scale bars, 0.25 cm.
Materials 14 03350 g009
Figure 10. Histological analysis of wounds treated with CaCO3, CaCO3-chitason and untreated wound as the control after 10 d stained with H&E (left) and Masson’s trichrome (right). Scale bar, 200 µm.
Figure 10. Histological analysis of wounds treated with CaCO3, CaCO3-chitason and untreated wound as the control after 10 d stained with H&E (left) and Masson’s trichrome (right). Scale bar, 200 µm.
Materials 14 03350 g010
Publisher’s Note: MDPI stays neutral with regard to jurisdictional claims in published maps and institutional affiliations.

Share and Cite

MDPI and ACS Style

He, W.; Huang, X.; Zhang, J.; Zhu, Y.; Liu, Y.; Liu, B.; Wang, Q.; Huang, X.; He, D. CaCO3–Chitosan Composites Granules for Instant Hemostasis and Wound Healing. Materials 2021, 14, 3350. https://doi.org/10.3390/ma14123350

AMA Style

He W, Huang X, Zhang J, Zhu Y, Liu Y, Liu B, Wang Q, Huang X, He D. CaCO3–Chitosan Composites Granules for Instant Hemostasis and Wound Healing. Materials. 2021; 14(12):3350. https://doi.org/10.3390/ma14123350

Chicago/Turabian Style

He, Wei, Xiaodong Huang, Jun Zhang, Yue Zhu, Yajun Liu, Bo Liu, Qilong Wang, Xiaonan Huang, and Da He. 2021. "CaCO3–Chitosan Composites Granules for Instant Hemostasis and Wound Healing" Materials 14, no. 12: 3350. https://doi.org/10.3390/ma14123350

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.

Article Metrics

Back to TopTop