Next Article in Journal
Regulation of the Gut Microbiota and Inflammation by β-Caryophyllene Extracted from Cloves in a Dextran Sulfate Sodium-Induced Colitis Mouse Model
Next Article in Special Issue
How Well Do We Handle the Sample Preparation, FT-ICR Mass Spectrometry Analysis, and Data Treatment of Atmospheric Waters?
Previous Article in Journal
Transformation of Residual Açai Fruit (Euterpe oleracea) Seeds into Porous Adsorbent for Efficient Removal of 2,4-Dichlorophenoxyacetic Acid Herbicide from Waters
Previous Article in Special Issue
Labeling Microplastics with Fluorescent Dyes for Detection, Recovery, and Degradation Experiments
 
 
Font Type:
Arial Georgia Verdana
Font Size:
Aa Aa Aa
Line Spacing:
Column Width:
Background:
Article

High-Pressure Supercritical CO2 Pretreatment of Apple Orchard Waste for Carbohydrates Production Using Response Surface Methodology and Method Uncertainty Evaluation

1
Research Institute for Analytical Instrumentation Subsidiary, National Institute for Research and Development for Optoelectronics Bucharest INOE 2000, 67 Donath Street, 400293 Cluj-Napoca, Romania
2
Faculty of Horticulture, University of Agricultural Sciences and Veterinary Medicine, 3-5 Manastur Street, 400372 Cluj-Napoca, Romania
*
Author to whom correspondence should be addressed.
Molecules 2022, 27(22), 7783; https://doi.org/10.3390/molecules27227783
Submission received: 14 October 2022 / Revised: 1 November 2022 / Accepted: 8 November 2022 / Published: 11 November 2022
(This article belongs to the Special Issue Advanced Analytical Techniques in Environmental Chemistry)

Abstract

:
This study’s objective was to separate cellulose, hemicellulose, and lignin after high-pressure supercritical carbon dioxide pretreatment for further valorization. The study investigated the supercritical carbon dioxide pretreatment of apple orchard waste at temperatures of 160–200 °C, for 15–45 min, at a pressure of 10 MPa. Response Surface Methodology (RSM) was used to optimize the supercritical process and to improve its efficiency. The change of functional groups during different pretreatment conditions was examined by Fourier transform infrared (FTIR) spectroscopy. Scanning electron microscopy (SEM) and X-ray diffraction (XRD) confirmed the structural changes in the biomass structure before and after pretreatment. A new ultra-high performance liquid chromatography (UHPLC) coupled with an evaporative light scattering detector (ELSD) method was developed and validated for the determination of carbohydrates in the liquid fraction that resulted after pretreatment. The estimated uncertainty of the method ranged from 16.9 to 20.8%. The pre-treatment of high-pressure supercritical CO2 appears to be an effective and promising technique for the recovery of sugars and secondary by-products without the use of toxic solvents.

1. Introduction

Agricultural activities generate large quantities of waste worldwide. Apple production and processing generates wastes, including pruning branches, spoiled apples, and pomace [1,2]. Previous research reported the use of lignocellulosic biomass as raw material for the production of ethanol using carbohydrate fermentation, biogas, or fuel for vehicles with fast pyrolysis [3,4]. In recent years, lignocellulosic biomass has been used to separate carbohydrates and convert them into value-added products, such as lactic acid [5]. Lignocellulosic biomass includes wood biomass, residues from forestry operations, agricultural wastes generated by various agricultural activities, and post-harvesting processes [6,7]. Lignocellulosic materials consist of cellulose, hemicellulose, and lignin, which are linked together to form a complex structure. Cellulose is a B-d-glucose homopolymer in which B-1-4-glycoside bonds connect the structural units. Hemicelluloses are polysaccharides consisting of pentoses (xylose and arabinoses), hexoses (mannose, glucose, and galactose), and uronic acids. Hemicelluloses establish hydrogen bonds with cellulosic microfibrils [8]. Due to its branched structure, hemicellulose is relatively easy to hydrolyze. The most critical step in separating important components from lignocellulosic biomass is pretreatment [9].
The separation efficiency of biomass components depends on the pretreatment method used. Supercritical carbon dioxide (CO2) is a widely used pretreatment method due to its moderate critical conditions (31.1 °C and 74 bar). The efficiency of supercritical CO2 pretreatment depends on temperature, time, and pressure. The mechanism involves the formation of hydrogen bonds that act as a Lewis acid and base. It is recommended to use a co-solvent to increase its polarity. The presence of moisture content and CO2 can generate carbonic acid which enhances the hydrolysis of hemicellulose in the liquid phase. Cellulose is soluble in ionic liquid and can precipitate in amorphous form by adding a nonsolvent, such as water or ethanol [10,11,12,13]. Jogi et al. [14] used supercritical ethanol to separate phenolic monomers from birch wood by using the following conditions: 243 °C and 63 bar pressure, 10% moisture content, and iron-based catalysts (5% Fe-SiO2).
The response surface methodology (RSM) model can be used to predict the optimal conditions in the variation of different variables. Pinto et al. [15] used RSM for the analysis of the oxypropylation process of lignocellulosic material. Wang et al. [16] reported studies about the use of RSM to optimize the ultrasound-assisted xanthation of cellulose from lignocellulosic biomass for further Pb adsorption. The model used was a Box–Behnken design and it fitted the experimental data and the verification of the variance analysis. Pandey et al. [17] studied the impact of surfactant-assisted acid and alkali pretreatment on lignocellulosic structure and optimization of saccharification parameters by using RSM. Gundapalli et al. [18] investigated the hydrothermal pretreatment of sugarcane bagasse for hemicellulose and lignin separation and used RSM for selecting the optimal operating conditions (water loading and time) in order to increase the digestibility of cellulose.
Several techniques are presented in the literature to analyze carbohydrates separated from lignocellulosic biomass, such as liquid chromatography coupled with a refractive index detector or mass spectrometry, gas chromatography, and UV-VIS spectrophotometry. Generally, the limit of detection (LOD) and limit of quantification (LOQ) is reported, but the uncertainty of the methods is not given [19,20,21]. In this context, the study aimed to develop and evaluate the uncertainty of the ultra-high performance liquid chromatography–evaporative light scattering detector (UHPLC–ELSD) method for the analysis of sugars resulting from the supercritical pretreatment of apple orchard waste (AOW).
The main objectives of the current research were: (i) the application of pretreatment with supercritical fluids assisted by CO2 for the separation of cellulosic components; (ii) the improvement of supercritical pretreatment conditions in order to find the optimal conditions through the use of the RSM; (iii) the spectroscopic investigation of raw material, before and after pretreatment by using SEM, XRD, and FTIR techniques; and (iv) uncertainty evaluation of a new analytical method for the analysis of carbohydrates in the hemicellulosic fraction using the UHPLC–ELSD method.

2. Results and Discussion

2.1. Chemical Composition of Apple Orchard Waste

The chemical compositions of apple orchard waste (AOW) were determined, and the results are presented in Table 1. The AOW contains 58.7% carbohydrates with high cellulose content (32.2 ± 0.07%). The moisture content was 6.96 ± 0.03%, and the total solids were 88.5%. The results showed a high cellulose content (32.2 ± 0.07%) of the AOW.

2.2. High-Pressure Supercritical CO2 Extraction of AOW

After pretreatment, two phases are formed: the solid phase, which contains cellulose, lignin, and a small amount of hemicellulose; and the liquid phase, which contains monomer sugars, oligomer sugars, and degradation products. The impact of temperature and time of the supercritical process on the AOW conversion of the solid yield and the chemical composition of each phase was studied. The mechanism of AOW supercritical pretreatment involves the following steps: the formation of strong hydrogen bonds with water that migrates on the surface of solid particles, chemosorption on the solid surface, the reaction of hydrogen ions (protons) and xylan at the surface, desorption of xylooligomers or splitting and diffusion of xylooligomers, and transport in the liquid phase.
The composition of the solid fraction after each experiment is presented in Table 2. The solid yield of the solid fraction recovered after the supercritical pretreatment ranges between 72.6–49.3%. It decreases with the increase in temperature and reaction time and it is mainly due to the solubilization of hemicelluloses in the liquid fraction. The composition of the solid fraction was analyzed after each experiment to determine the cellulose, hemicellulose, and lignin content. The cellulose content varies between 37.2–47.2 g/100 g pretreated AOW, and the lignin content varies between 33.0–44.8 g/100 g pretreated AOW. The content of hemicellulose decreases with the increase in temperature and reaction time (from 15 min to 45 min); at 200 °C, hemicelluloses are hydrolyzed almost completely in the liquid fraction. The cellulose and lignin content increase explains its low degradation in supercritical fluids. The amount of cellulose recovered in the solid fraction was high. Lignin has a similar behavior, depending on the temperature and reaction time.
Optimum Condition of the Supercritical CO2 Method for Extracting Cellulose Designed by the Response Surface Methodology (RSM).
The RSM technique was used as a statistical tool to evaluate the supercritical pretreatment method [22]. The obtained plots for solid yield, cellulose, hemicellulose, and lignin are presented in Figure 1, Figure 2, Figure 3 and Figure 4. This model evaluates the optimal conditions for the pretreatment to obtain high cellulose content in the solid fraction. The cellulose will be further hydrolyzed and the obtained sugars will be the substrate for bioplastic production.
Based on the contour plots, the theoretical results for solid yield, cellulose, hemicellulose, and lignin content versus temperature and time are presented in Table 3, Table 4, Table 5 and Table 6. The p-value was used to observe the significance of the model The degree of freedom is the number of independent variables. The temperature has a low p-value of < 0.05 in all experiments, indicating a very high significance. A second-order polynomial was used to measure the correlation between the response and the independent variables.
The analysis of the RSM model for solid yield, cellulose, hemicellulose, and lignin content was verified by measuring the R2 coefficient (Table 7). A lack of fit test was carried out. The p-values for the lack of fit were <0.05 for solid yield, hemicellulose, and lignin content. The F values were relatively higher than the 95% confidence level, indicating that the model is significant. The higher F suggested that the model is significant for these parameters.
The regression equations (Equations (1)–(4)) are presented below:
Solid yield (%) = 509 − 4.48 X1 − 0.794 X2 + 0.01137 X12 + 0.00556 X22 + 0.00067 X1X2
Cellulose = −468.6 + 5.641X1 − 0.703 X2 − 0.01525 X12 + 0.00933 X22 + 0.000917 X1X2
Hemicellulose = 264.5 − 2.51 X1 − 0.339 X2 + 0.00592 X12 − 0.01794 X22 + 0.000608 X1X2
Lignin = −72.3 + 0.896X1 + 0.264 X2 − 0.001508 X12 − 0.00397 X22 − 0.001083 X1X2
The model indicates that temperature and time significantly affect the content of cellulose, hemicellulose, and lignin. The R2 value ranged between 93.55% and 95.45%, indicating that the proposed model reasonably adjusted the empirical data. The value of R2 must be close to 1 for an ideal model. The model has an R2 higher than 93% in all the experiments and the low standard deviation proved the accuracy of the model.
Table 8 presents the optimal solution predicted by the model for each measured parameter. The optimal parameters for obtaining the highest cellulose content are a temperature of 185.8 °C and a reaction time of 45 min. The experimental data obtained after applying the optimum solutions confirm that the experimental and estimated values are close. Becze et al. used a high-pressure extraction process of antioxidant compounds from Feteasca regala using RSM, and the values obtained in experiments were confirmed by the RSM model [23]. Wang et al. [16] also used RSM for cellulose content obtained from lignocellulosic biomass by using an ultrasound-assisted pretreatment method. The Box–Behnken design was used.
Based on the results obtained, it can be concluded that RSM is suitable for setting the conditions for improving cellulose production from AOW using high-pressure CO2 pretreatment. The model indicated that the temperature and pretreatment time were significant for the content of the compounds that resulted after pretreatment in the solid fraction.

2.3. Method Validation and Uncertainty Evaluation for Sugars Analysis by UHPLC-ELCD Detector

The simultaneous analysis of five sugars (xylose, arabinose, mannose, glucose, galactose) from the hemicellulosic fraction separated after the pretreatment of the AOW samples using the UHPLC–ELSD method was developed and validated.
The ELSD performance parameters were optimized to obtain good sensitivity and separation of C5 and C6 sugars. The nebulization temperature, evaporation, and gas flow were tested to obtain the separation of sugars. At a temperature of 70 °C for nebulization and 90 °C for evaporation, the complete separation of sugars was obtained. The unseparated sugars were obtained via nebulization and evaporation at 90 °C. Another factor that affected the separation was the temperature of the chromatographic column. The total time of analysis was 20 min, but in the first eight minutes, the separation of the analyzed sugars occurred. An injection volume of 20 µL provided the best response. Method validation in terms of linearity, detection limit, quantitation limit, accuracy, reproducibility, and recovery was conducted according to the requirements of the EURACHEM Guide [24]. The chromatographic separation of carbohydrates in the sample analysis (conditions T = 200 °C for 45 min) is presented in Figure 5.
Selectivity was demonstrated by evaluating the retention time of blank samples enriched with a known concentration of sugars. The reproducibility was determined by evaluating the retention time variation (%CV). The reproducibility was less than 0.5% in the case of each type of sugar (Table 9). The linearity, LOD, LOQ, and R2 obtained for each sugar are presented in Table 9, while the statistical parameters of the calibration curve are given in Table 10. The concentration range for each sugar was 25 (LOQ)−250 µg mL−1.
The bottom-up approach was taken into account for calculating the uncertainty. The primary sources of uncertainty contributing to the method are the purity of the standards, the analytical balance used for the preparation of stock solutions, the volumetric flask, pipettes used for the preparation of working solutions, the equipment, the calibration curve, and the repeatability of the method. The purity of the reference material was specified in the quality certificate of the standard. As the quality certificate of the reference material does not specify the uncertainty type, a rectangular distribution of the uncertainty distribution is considered; thus, the uncertainty is divided by a radical of three to transform it into standard uncertainty. The uncertainty of the analytical balance was obtained by composing the uncertainty given by an accredited testing laboratory, and the repeatability standard deviation was used. The following factors were considered for the calculation of the uncertainty of the micro-pipettes: calibration certificate, uncertainty of pipetting at different temperatures, and repeatability. The precision was defined as the standard deviation of the response obtained from the measurement of six parallel samples. Sx0 gave the uncertainty of the calibration curve calculated as the ratio between the residual standard deviation (Sy) and the slope (b). The precision was also evaluated as the relative standard deviation (RSD). The expanded uncertainty was calculated considering a cover factor k = 2 for a level of confidence of 95% (Table 11). The PG values are accepted because they are lower than the Fisher–Snedecor distribution.
The method developed for the analysis of sugars demonstrated excellent precision and can be used for the analysis of sugars from hemicellulosic fractions obtained after pretreatment.

2.3.1. Chemical Composition of Liquid Samples

The influence of temperature and reaction time on sugar content in a liquid fraction that resulted after pretreatment is presented in Table 12. The results in this study are reported with the expanded uncertainty (k = 2) for sugar analysis and standard deviation for furfural and 5-hydroxymethylfurfural (HMF) content.
The composition of the sugars in the filtrate recovered after pretreatment shows that pentoses are much more sensitive to water and CO2 treatment under the pretreatment conditions compared with hexose sugars (glucose, mannose, and galactose). The results show a higher arabinose content than other sugar types. The sugars that resulted after the hydrolysis of hemicelluloses are mainly pentoses (xylose and arabinose). After the AOW pretreatment, about 7% of sugars were obtained for the pretreatment performed at 160 °C, 10% at 180 °C, and 8% at 200 °C. For the same reaction time, the sugar concentration increases as the temperature increases. This occurs until a reaction time of 30 min, after which it begins to decrease up to a 45 min reaction time. Alinia et al. [25] obtained the best overall yields for sugar (208 g kg−1) with supercritical CO2 pretreatment at 185 °C for a 30 min reaction time for wheat straw. The proposed mechanism for the transformation of hexoses into HMF is presented in Figure 6.
The decrease in the 5-HMF concentration could be attributed to the polymerization and hydrolysis of 5-HMF at high temperatures, as well as the production of levulinic acid, humins, and formic acid [26]. The highest furfural content was produced by pretreatment performed at 160 °C for 45 min. The furfural content decreased at high temperatures and time. A possible explanation could be the boiling of furfural at 162 °C. According to Yong et al. [27], supercritical fluid extraction enhances the depolymerization of pentosan. The dissolution of carbon dioxide leads to the formation of carbonic acid which favors acidic conditions for bonding cleavages. Furfural is formed from pentoses contained in the hemicellulose phase. Further, furfural can be extracted from the liquid phase with a solvent (ex. toluene) and used as a chemical. The obtained results suggested that AOW can be a good source for obtaining furfural. Binder et al. [28] obtained furfural from the agricultural residue by converting xylose to furfural with a conversion yield of 53%.

2.3.2. Optimum Condition of the Pretreatment Method for Extracting Sugars in Liquid Fraction Designed by RSM

The final compositions of the sugars were optimized using response surface methodology. The response plot for xylose vs. two different input variables (temperature and time) is presented in Figure 7.
The multiple regression for xylose (Table 13) and the summary reports for the other sugars are presented in Equations (5)–(9).
The regression equations (Equations (5)–(9)) are presented below:
Xylose (µg mL−1) = −3329 + 36.9 X1 + 54.9 X2 −0.1011 X12 −0.79 X22 − 0.022 X1X2
Arabinose (µg mL−1) = −6498 + 72.1 X1 + 77.1 X2 − 0.1981 X12 − 1.124 X22 − 0.0314 X1X2
Mannose (µg mL−1) = −702 + 8.56 X1 + 17.81 X2 − 0.0253 X12 − 0.3212 X22 − 0.0164 X1X2
Glucose (µg mL−1) = −1110 + 12.60 X1 + 5.5 X2 − 0.035 X12 − 0.0862 X22 − 0.00164 X1X2
Galactose (µg mL−1) = −901 + 10.26 X1 + 12.18 X2 − 0.0286 X12 − 0.1990 X22 − 0.00417 X1X2
The p-value was used to test the significance of the model for the predicted sugars (Table 14). The lack of fit (in all cases) was smaller than p < 0.05, proving that the model was significant.
The values of the coefficient of variation for all parameters show a good fit of the model with the experimental data at a 95% confidence level. The calculated F values (6.85—xylose, 7.64—arabinose, 1.72—mannose, 2.37—glucose, and 2.30—galactose) proved that the model was sufficiently significant. The model can be used only for the fit data between the variables’ minimum and maximum values. The pretreatment temperature was the factor that had the most significant influence on the content of sugars in the hemicellulosic fraction.

2.4. Structural Characterization of the AOW before and after Pretreatment

2.4.1. SEM Analysis

To evaluate the structural modification of AOW before and after pretreatment at each temperature, SEM imagining was carried out. In SEM images of raw material, a compressed structure can be observed. During the temperature increase, the fibers are broken and the cellulose structure can be observed. The structure of treated AOW (Figure 8b–d) may be due to the solubilization of hemicellulose in the liquid fraction [29]. The use of water as a co-solvent can create an equilibrium, and some parts of the water’s CO2 cannot dissolve it.
The SEM images of the AOW differ depending on the temperature applied to the pretreatment.

2.4.2. FTIR Spectra

The FTIR spectra for the raw and pretreated apple orchard waste is presented in Figure 9.
Fourier transform infrared spectroscopy (FTIR) was used to analyze untreated and pretreated AOW. IR spectroscopy studies provide information on the functional groups present in the structure of raw material and can provide information on changes in the functional groups before and after the pretreatment method. Figure 9b presents the functional groups for the cellulose standard revealing the following band assignments: 3400 cm−1 is the OH-stretching vibrations range, 2800 cm−1 is CH and CH2 stretching, 1500 cm−1 is the COH and HCH bending, 1400 cm−1 is the CH and COH bending, 1200 cm−1 is skeletal vibrations of C-O-C stretching, and 1000 cm−1 is the vibration of C-O and ring stretching. The vibration presented at 1739 cm−1 was attributed to the valence vibration of the C=O group from hemicellulose. This band almost disappears in the spectrum of treated raw material at different temperatures. The adsorption peaks of lignin were around 1624, 1515, and 1455 cm−1. The band at 1371 cm−1 was attributed to vibrations of C-H from cellulose. The band at around 1317 cm−1 was assigned to C-H vibration from cellulose and hemicellulose. The 1059 cm−1 band was caused by CH in plain deformation of C-O from cellulose and hemicellulose. The bands presented at 1427, 1371, 1160, and 1032 cm−1 are valence vibrations of cellulose (Figure 9b). There is a visible difference in the FTIR spectrum of the untreated and pretreated AOW, as shown by the absence of adsorption bands or by changing the intensity and profile of certain bands [30].

2.4.3. XRD Analysis

The X-ray diffraction patterns of the raw and pretreated AOW are presented in Figure 10.
Lignocellulosic biomass is mainly composed of polysaccharides (cellulose and hemicellulose) and lignin. Hemicellulose and lignin are amorphous, while cellulose has both amorphous and crystalline components [31]. The XRD technique offers information on the crystalline content. The main crystalline and amorphous peaks arise around 2θ = 22° and between 2θ values of 15 and 18°, respectively. Two typical diffraction peaks were observed at approximately 15° and 22°, corresponding to the lowest (101) and highest (002) peaks, indicating that type I cellulose was the main form of cellulose in the investigated sample [32]. The peak intensity increases and peaks become narrower with the increase in the pretreatment temperature. The relative fraction of the crystalline component in the cellulose is expressed as the crystallinity index (CrI), calculated according to the Segal empirical equation [33]. The Segal formula is one of the most used techniques for calculating the crystallinity index at the peak height of crystalline materials. The CrI values varied in the following order: 51.4% (raw) < 51.7 (160 °C) < 54.5 (180 °C) < 56.6 (200 °C). The enhanced crystallinity indicates the removal of hemicellulose and lignin [34].

3. Materials and Methods

3.1. Chemicals and Reagents

All used chemicals were of analytical reagent grade. Acetic acid, dichloromethane, sulfuric acid (98%), sodium hydroxide, methanol, hydrochloric acid, ethanol, toluene, acetone, acetonitrile, and CO2 (≥99.8%) were purchased from Merck (Darmstadt, Germany). 5-hydroxymethylfurfural (HMF) and furfural were purchased from Sigma-Aldrich (St. Louis, MO, USA). Standards of D(+)-glucose (99.5%), D(+)-mannose (99.0%), D(+)-galactose (99.0%), D(−)-arabinose (98.0%), D(+)-xylose (990%) were purchased from Merck (Darmstadt, Germany). Sodium chlorite (80%) was purchased from Alfa Aesar GmbH & Co (Karlsruhe, Germany). All solutions were prepared by using ultrapure water (18.2 MΩcm−1 at 20 °C) obtained from a Direct-Q3 UV Water Purification System (Millipore, Molsheim, France).

3.2. Sample Description

The AOW samples were purchased from the Research Station of the University of Agricultural Sciences “Ion Ionescu de la Brad” from Iași, farm no. 3 “Vasile Adamachi” (Romania). The samples were collected immediately after the cutting operations of apple trees, and they were dried and shredded to a diameter of 0.2 mm.

3.3. High-Pressure Supercritical CO2 Pretreatment

The AOW was pretreated by supercritical CO2 pretreatment using a steel pressure Parr reactor (Parr Instruments, Moline, IL, USA), equipped with a Parr 4523 temperature controller and a 1 L reaction vessel. Approximately 30 g of biomass was placed into the reactor vessel with 300 mL water, and then the mixtures were placed in the autoclave reactor. The reactor contains the following components: an external controller, thermocouple, magnetic stirring system, heating jacket, pressure gauge, gas inlet, pressure valve, and CO2 cylinder pressure at 25 °C (6.8 MPa). The CO2 amount was introduced in the reactor by using a restrictor valve until the desired pressure (10 MPa), to ensure that only liquid carbon dioxide was present. During the reaction process, stirring was set at 600 rpm to allow better mixing of biomass with CO2. The reactor was tightly sealed and heated to a set temperature (160, 180, and 200 °C) and time (15, 30, and 45 min) with a ramp-up time of a few minutes to reach the desired parameters. Pressure increased once the reactor was heated up, and the volume of CO2 varied with temperature. After the test was finished, the CO2 gas was slowly released using a pressure valve, the heating was stopped, and the reaction vessel was cooled at room temperature. The heating and cooling time varied in each experiment (for the experiment, −200 °C and 45 reaction time); the heating time was 30 min to ensure the equilibrium. The samples were cooled at room temperature, the solid fraction was separated by filtration, and the chemical composition of solid and liquid fractions was determined. The liquid samples were recovered and analyzed for sugar content.

RSM Methodology

RSM is used to predict the influence of temperature and time (variables) on cellulose content, hemicellulose content, yield, and solid composition (independent variables) in supercritical CO2 pretreatment. The Minitab software was used to optimize the RSM model. The water was chosen as a co-solvent to help the separation. In the supercritical pretreatment of the AOW, the dependent variables were the content of cellulose, hemicellulose, lignin, and solid yields, and the dependent variables were temperature and time. The mathematical model used is detailed in the study conducted by Pinto et al. [15]. The effect of temperature (X1) and time (X2) on the solid fraction composition that resulted after the supercritical pretreatment was investigated using full factorial. All experiments were conducted in triplicate. Two independent variables were studied at three different levels (Table 15). The central composite design (CCD) was used as a type of response surface modeling. The CCD design was carried out with three levels for individual variables X1 and X2. The second-order polynomial equation used was presented in Equation (10):
Y= β 0 + J = 1 k = 2 β j   x j + J = 1 k = 2 β jj   x j 2 + J = 1 k = 2 β jj   x i x j + Є  
where β0 and βii are the regression coefficients; Xi, Xii, and XiXj are the main, interaction, and quadratic terms, respectively; Y is the responsible variable; k is the number of independent variables.
Optimal conditions were applied in order to verify the model by comparing experimental and predicted values.

3.4. Analytical Characterization

3.4.1. Chemical Characterization of Raw and Pretreated Biomass

Ash and moisture were analyzed gravimetrically. The moisture content was determined by drying for 24 h at 105 °C in an oven (Memmert Tip UFE 400 GmbH + Co. KG, Schwabach, Germany) to a constant weight. The ash content was determined after the incineration of samples at 550 °C according to ASTM D1102-84 (2021) [35]. The extractables were determined by extracting the sample with ethanol in a Soxhlet extractor for 6 h. The elemental analysis was determined by a Flash EA 2000 CHNS/O analyzer (Thermo Fisher Scientific, Waltham, MA, USA) [36,37,38]. The content of cellulose, hemicellulose, and lignin was determined according to Teramoto et al. [39]. The holocellulose was determined by the reaction of raw material with NaClO2 at 75 °C for 1 h. The cellulose was obtained by the reaction of the previously obtained holocellulose with 17.5% NaOH at 20 °C for 40 min. The hemicellulose content was calculated as the difference between the amount of holocellulose and cellulose. The lignin content was determined as insoluble residue that resulted after the reaction of raw material with 72% H2SO4.

3.4.2. Chemical Analysis of Sugars Obtained in Liquid Samples

UHPLC (Agilent Technologies, Santa Clara, CA, USA) was used to analyze the liquid fraction that resulted after pretreatment for monosaccharides (glucose, mannose, galactose, xylose, and arabinose), HMF, and furfural. The content of mono-sugars was analyzed by UHPLC (1260 Infinity II), which contains a quaternary pump (Agilent Technologies, G7111B, 1260 Infinity II, Santa Clara, CA, USA), an Agilent Autosampler with an injection valve fitted with a 20 µL sample loop. The separation was performed on a 5 µm Polaris NH2 250 × 4.6 mm (Agilent Technologies, Santa Clara, CA, USA). The column temperature (Agilent Technologies 1290 Infinity II Multicolumn Thermostat, Santa Clara, CA, USA) was kept constant at 30 °C, and the mobile phase flow rate was 0.6 mL.min−1. The Evaporative Light Scattering Detector (ELSD) (Agilent Technologies, 1290 Infinity ELSD, Santa Clara, CA, USA) has the following characteristics: nebulization temperature of 70 °C, evaporation temperature of 90 °C, and gas flow of 1.2 SLM. The eluent used was acetonitrile: water (75:25) with a flow rate of 0.6 mL min−1 and an injection volume of 20 µL. All the samples were filtered through a 0.45 µM PTFE filter for LC analysis.
The content of furfural and HMF was analyzed according to our recent methods published [40,41].

3.4.3. Strategy for Methods’ Validation

The standards were dissolved in ultrapure water. The working solutions were prepared in eluent (75:25 ACN:water (v/v)) and used for the UHPLC analysis. The calibration curve was prepared with six appropriate concentrations for each analyte (25, 50, 100, 150, 200, and 250 µg mL−1). The stock solutions were diluted with eluent (75:25 ACN:water (v/v)) and filtered through a 0.45 µm membrane. The limit of detection (LOD) was calculated as 3 × standard deviations of the response given by the analysis of six blank replicates, while the limit of quantification (LOQ) was calculated as 3 × LOD. The precision in the samples was determined at four different spiked concentrations of sugars (25, 100, 200, and 250 µg mL−1) and evaluated as relative standard deviations. The homogeneity of the dispersion was evaluated as PG and calculated as a ratio between the standard deviation of the lowest and the highest limits.
The uncertainty measurement was carried out according to the EURACHEM guide [24]. The uncertainty was reported as expanded uncertainty; calculated as Urel = k × Uc, where k = 2 is the coverage factor (for a level of confidence of 95%); and Uc was the combined standard uncertainty.

3.5. Structural Characterization

3.5.1. Scanning Electron Microscopy (SEM)

The AOW samples, before and after pretreatment, were examined using a scanning electron microscope (SEM VEGAS 3 SBU, Tescan, Brno-Kohoutovice, Czech Republic) with a Quantax EDS XFlash (Bruker, Karlsruhe, Germany) detector. The samples were deposited on a double-sided conductive carbon tape on two aluminum stubs and analyzed.

3.5.2. X-ray Diffraction (XRD)

The X-ray diffraction (XRD) patterns were performed using a D8 Advance diffractometer (Bruker, Karlsruhe, Germany), operating at 40 kV and 35 mA, with CuKα radiation (λ = 1.5406 Å), at room temperature. The crystallinity index (CrI) was calculated using the Segal empirical equation (Equation (11)) via a maximum intensity of the 200 lattice diffraction peak (I002, 2θ ≈ 22.5°) and the minimum intensity of the diffraction between the 002 and 110 peaks (Iam, 2θ ≈ 18°) that correspond to amorphous cellulose.
CrI (%) = (I002 − Iam)/I002 × 100

3.5.3. FTIR Analysis

The FTIR spectra of raw and pretreated AOW were recorded using a Spectrum BX II (Perkin Elmer, Waltham, MA, USA) spectrometer in the range of 4000–400 cm−1 on 1% KBr pellets with a spectral resolution of 2 cm−1, in order to identify different functional groups and monitor changes occurring at the functional groups level during different conversion processes.

4. Conclusions

This study investigated the influence of high-pressure supercritical CO2 pretreatment on apple orchard waste for separating sugars into cellulosic and hemicellulosic fractions. The contents of solid and liquid fractions that resulted after pretreatment were evaluated. The results obtained in the experiments were compared with the expected results obtained using the RSM model. A new method of sugar analysis has been developed by using the UHPLC-ELSD method. This method is environmentally friendly due to the low consumption of organic solvents and the absence of the extraction step before injection. The uncertainty of the method was calculated for each type of sugar based on a bottom-up approach. The obtained sugars can be used as raw material to produce bioplastics by using specific strains.

Author Contributions

Conceptualization, L.S.; methodology, D.A.S., E.A.L., O.C., A.B. and C.V., software, D.A.S.; validation, L.S.; formal analysis, O.C., E.A.L. and A.B.; investigation, C.V.; resources, L.S.; data curation, D.A.S.; writing—original draft preparation, L.S.; writing—review and editing, L.S. and E.K.; visualization, O.C. and E.A.L.; supervision, L.S.; project administration, L.S.; funding acquisition, L.S. All authors have read and agreed to the published version of the manuscript.

Funding

This work was supported by a grant from the Ministry of Research, Innovation and Digitization, CNCNS-UEFISCDI, project number PN-III-P1.1.1-TE-2021-0179, within PNCDI III, LIGNOBIOPLAST.

Institutional Review Board Statement

Not applicable.

Data Availability Statement

Not applicable.

Conflicts of Interest

The authors declare no conflict of interest.

Sample Availability

Samples are available from the authors.

References

  1. Caldeira, C.; Vlysidis, A.; Fiore, G.; Laurentiis, V.D.; Vignali, G. Sustainability of food waste biorefinery: A review on valorization pathways, techno-economic constraints. Bioresour. Technol. 2020, 312, 123575. [Google Scholar] [CrossRef] [PubMed]
  2. Dyjakon, A. The influence of apple orchard management on energy performance and pruned biomass harvesting for energetic applications. Energies 2019, 12, 632. [Google Scholar] [CrossRef] [Green Version]
  3. Bhatia, S.K.; Jagtap, S.S.; Bedekar, A.A.; Bhatia, R.K.; Rajendran, K.; Pugazhendhi, A.; Rao, C.V.; Atabani, A.E.; Kumar, G.; Yang, Y.H. Renewable biohydrogen production from lignocellulosic biomass using fermentation and integration of systems with other energy generation technologies. Sci. Total Environ. 2021, 765, 144429. [Google Scholar] [CrossRef]
  4. Pocha, C.K.R.; Chia, S.R.; Chia, W.Y.; Koyande, A.K.; Nomanbhay, S.; Chew, K.W. Utilization of agricultural lignocellulosic wastes for biofuels and green diesel production. Chemosphere 2022, 292, 133246. [Google Scholar] [CrossRef] [PubMed]
  5. Esquivel-Hernández, D.A.; García-Pérez, J.S.; López-Pacheco, I.Y.; Hafiz, M.; Iqbal, N.; Parra-Saldívar, R. Resource recovery of lignocellulosic biomass waste into lactic acid-Trends to sustain cleaner production. J. Environ. Manag. 2022, 301, 113925. [Google Scholar] [CrossRef]
  6. Kawaguchi, H.; Takada, K.; Elkasaby, T.; Pangestu, R.; Totoshim, M.; Kadar, P.; Ogino, C.; Kaneko, T.; Kondo, A. Recent advances in lignocellulosic biomass white biotechnology for bioplastics. Bioresour. Technol. 2022, 344, 126165. [Google Scholar] [CrossRef] [PubMed]
  7. Qin, S.; Giri, B.S.; Patel, A.K.; Sar, T.; Liu, H.; Chen, H.; Juneja, A.; Kumar, D.; Zhang, Z.; Awasthi, M.K.; et al. Resource recovery and biorefinery potential of apple orchard waste in the circular bioeconomy. Bioresour Technol. 2021, 321, 124496. [Google Scholar] [CrossRef]
  8. Montroni, D.; Giosia, M.D.; Falini, G. Supramolecular binding with lectins: A new route for non-covalent functionalization of polysaccharide matrices. Molecules 2022, 27, 5633. [Google Scholar] [CrossRef]
  9. Zabed, H.; Sahu, J.N.; Boyce, A.N.; Faruq, G. Fuel ethanol production from lignocellulosic biomass: An overview on feedstocks and technological approaches. Renew. Sustain. Energy Rev. 2016, 66, 751–774. [Google Scholar] [CrossRef]
  10. Sun, J.; Ding, R.; Yin, J. Pretreatment corn ingredient biomass with high pressure CO2 for conversion to fermentable sugars via enzymatic hydrolysis of cellulose. Ind. Crops Prod. 2022, 177, 114518. [Google Scholar] [CrossRef]
  11. Seoud, O.A.E.; Kostag, M.; Jedvert, K.; Malek, N.I. Cellulose in ionic liquids and alkaline solutions: Advances in the mechanisms of biopolymer dissolution and regeneration. Polymers 2019, 11, 1917. [Google Scholar] [CrossRef] [PubMed] [Green Version]
  12. Zhao, M.J.; Xu, Q.Q.; Li, G.M.; Zhang, Q.Z.; Zhou, D.; Yin, J.Z.; Zhan, H.S. Pretreatment of agricultural residues by supercritical CO2 at 50–80 °C to enhance enzymatic hydrolysis. J. Energy Chem. 2019, 31, 39–45. [Google Scholar] [CrossRef] [Green Version]
  13. Ran, F.; Wang, X.; Li, H.; Zhang, H.; Pang, J.; Wang, Z.; Li, L. High yield of reducing sugar from enzymolysis of cellulose in supercritical carbon dioxide system. Ind. Crops Prod. 2022, 178, 114632. [Google Scholar] [CrossRef]
  14. Jogi, R.; Maki-Arvela, P.; Virtanen, P.; Kumar, N.; Hemming, J.; Russo, V.; Samikannu, A.; Lestander, T.A.; Mikkola, J. Understanding the formation of phenolic monomers during fractionation of birch wood under supercritical ethanol over iron based catalysts. J. Energy Inst. 2020, 93, 2055–2062. [Google Scholar] [CrossRef]
  15. Pinto, J.A.; Prieto, M.A.; Ferreira, I.C.F.R.; Belgacem, M.N.; Rodriques, A.E.; Barreiro, M.F. Analysis of the oxypropylation process of a lignocellulosic material, almond shell, using the response surface methodology (RSM). Ind. Crops Prod. 2020, 153, 112543. [Google Scholar] [CrossRef]
  16. Wang, C.; Wang, H.; Gu, G. Ultrasound-assisted xanthation of cellulose from lignocellulosic biomass optimized by response surface methodology for Pb (II) sorption. Carbohydr. Polym. 2018, 182, 21–28. [Google Scholar] [CrossRef]
  17. Pandey, A.K.; Negi, S. Impact of surfactant assisted acid and alkali pretreatment on lignocellulosic structure of pine foliage and optimization of its saccharification parameters using response surface methodology. Bioresour. Technol. 2015, 192, 115–125. [Google Scholar] [CrossRef]
  18. Gundapalli, M.P.; Tantayotai, P.; Panakkal, E.J.; Chuetor, S.; Kirdponpattara, S.; Thomas, A.S.S.; Sharma, B.K.; Sriariyanum, M. Hydrothermal pretreatment optimization and deep eutectic solvent pretreatment of lignocellulosic biomass: An integrated approach. Bioresour. Technol. Rep. 2022, 17, 100957. [Google Scholar] [CrossRef]
  19. Tsai, Y.-H.; Tsai, C.-W.; Tipple, C.A. A validated method for the analysis of sugars and sugar alcohols related to explosive via liquid chromatography mass spectrometry (LC-MS) with post-column addition. Forensic Chem. 2022, 28, 100404. [Google Scholar] [CrossRef]
  20. Li, P.; Chatterjee, M.; Lämmerhofer, M. Targeted analysis of sugar phosphates from glycolysis partway by phosphate methylation with liquid chromatography coupled to tandem mass spectrometry. Anal. Chim. Acta 2021, 1221, 340099. [Google Scholar] [CrossRef]
  21. Hyvärinen, S.; Mikkola, J.P.; Murzin, D.Y.; Vaher, M.; Kaljurand, M.; Koel, M. Sugars and sugar derivatives in ionic liquid media obtained from lignocellulosic biomass: Comparison of capillary electrophoresis and chromatographic analysis. Catal. Today 2014, 223, 18–24. [Google Scholar] [CrossRef]
  22. Muhammad, G.; Ngatcha, A.D.P.; Xiong, W.; El-Badry, Y.; Asmatulu, E.; Xu, J.; Alam, M.A. Enhanced biodiesel production from wet microalgae biomass optimized via response methodology and artificial neural network. Renew. Energy 2022, 184, 753–764. [Google Scholar] [CrossRef]
  23. Becze, A.; Babalau-Fuss, V.L.; Varaticeanu, C.; Roman, C. Optimization of high-pressure extraction process of antioxidant compounds from Feteasca regala leaves using Response Surface Methodology. Molecules 2020, 25, 4209. [Google Scholar] [CrossRef] [PubMed]
  24. EURACHEM. CITAC Guide CG4, Quantifying Uncertainty in Analytical Measurement, 3rd ed.; Ellison, S.L.R., Williams, A., Eds.; Eurachem: Teddington, UK, 2012; pp. 1–132. [Google Scholar]
  25. Alinia, R.; Zabihi, S.; Esmaeilzadeh, F.; Kalajahi, J.F. Pretreatment of wheat straw by supercritical CO2 and its enzymatic hydrolysis for sugar production. Biosyst. Eng. 2010, 107, 61–66. [Google Scholar] [CrossRef]
  26. Ji, Q.; Jiang, H.; Yu, X.; Yagoub, A.E.G.; Zhou, C.; Chen, L. Efficient and environmentally-friendly dehydration of glucose and treatments of bagasse under the supercritical CO2 system. Renew. Energy 2020, 162, 1–12. [Google Scholar] [CrossRef]
  27. Yong, K.J.; Wu, T.Y.; Lee, C.B.T.L.; Lee, Z.J.; Liu, Q.; Jahim, J.M.; Zhou, Q.; Zhang, L. Furfural production from biomass residues: Current technologies, challenges and future prospects. Biomass Bioenerg. 2022, 161, 106458. [Google Scholar] [CrossRef]
  28. Binder, J.B.; Blank, J.J.; Cefali, A.V.; Raines, R.T. Synthesis of furfural from xylose and xylan. Chem.Sus.Chem. 2010, 3, 1268–1272. [Google Scholar] [CrossRef] [Green Version]
  29. Lü, H.; Ren, M.; Zhang, M.; Chen, Y. Pretreatment of corn stover using supercritical CO2 with water-ethanol as co-solvent. Chin. J. Chem. Eng. 2013, 21, 551–557. [Google Scholar] [CrossRef]
  30. Rahmani, A.M.; Gahlot, P.; Moustakas, K.; Kazmi, A.A.; Ojha, C.S.P.; Tyagi, V.K. Pretreatment methods to enhance solubilization and anaerobic biodegradability of lignocellulosic biomass (wheat straw): Progress and challenges. Fuel 2022, 319, 123726. [Google Scholar] [CrossRef]
  31. Taherzadeh, M.J.; Karimi, K. Pretreatment of lignocellosic wastes to improve ethanol and biogas production: A review. Int. J. Mol. Sci. 2008, 9, 1621–1651. [Google Scholar] [CrossRef]
  32. Senila, L.; Tenu, I.; Carlescu, P.; Scurtu, D.A.; Kovacs, E.; Senila, M.; Cadar, O.; Roman, M.; Dumitras, D.E.; Roman, C. Characterization of biobriquettes produced from vineyard wastes as a solid biofuel resource. Agriculture 2022, 12, 341. [Google Scholar] [CrossRef]
  33. Segal, L.; Creely, J.; Martin, A.; Conrad, C. An empirical method for estimating the degree of crystallinity of native cellulose using the X-ray difractometer. Text. Res. J. 1959, 29, 786–794. [Google Scholar] [CrossRef]
  34. Galiwango, E.; Rahman, N.S.A.; Al-Marzouqi, A.H.; Abu-Omar, M.M.; Khaleel, A.A. Isolation and characterization of cellulose and α-cellulose from date palm biomass waste. Heliyon 2019, 5, e02937. [Google Scholar] [CrossRef] [PubMed] [Green Version]
  35. Standard Test Method for Ash in Wood. ASTM D1102-84; ASTM International: West Conshohocken, PA, USA, 2021.
  36. ISO 10694:1995; Soil Quality—Determination of Organic and Total Carbon after Dry Combustion (Elementary Analysis). International Organization for Standardization: Geneva, Switzerland, 1995.
  37. ISO 13878:1998; Soil Quality—Determination of Total Nitrogen Content after Dry Combustion (Elementary Analysis). International Organization for Standardization: Geneva, Switzerland, 1998.
  38. ISO 15178:2000; Soil Quality—Determination of Total Sulfur by Dry Combustion. International Organization for Standardization: Geneva, Switzerland, 2000.
  39. Teramoto, Y.; Lee, S.; Endo, T. Pretreatment of woody and herbaceous biomass for enzymatic saccharification using sulphuric acid-free ethanol cooking. Bioresour. Technol. 2008, 99, 8856–8863. [Google Scholar] [CrossRef]
  40. Senila, L.; Scurtu, D.A.; Kovacs, E.; Senila, M.; Tomoiag, C.H.; Roman, C. Determination of furfural from vineyard waste by ultra-high performance liquid chromatography-diode array detection (UHPLC-DAD) with method validation and uncertainty evaluation. Anal. Lett. 2022, 55, 665–674. [Google Scholar] [CrossRef]
  41. Senila, L.; Gog, A.; Senila, M.; Roamn, C.; Silaghi-Dumitrescu, L. Development of a GC-MS method for 5-hydroxymethylfurfural determination in wood after steam-explosion pretreatment. Rev. Chim. 2012, 63, 557–561. [Google Scholar]
Figure 1. Contour plots of solid yield depending on time and temperature.
Figure 1. Contour plots of solid yield depending on time and temperature.
Molecules 27 07783 g001
Figure 2. Contour plots of cellulose content depending on time and temperature.
Figure 2. Contour plots of cellulose content depending on time and temperature.
Molecules 27 07783 g002
Figure 3. Contour plots of hemicellulose content depending on time and temperature.
Figure 3. Contour plots of hemicellulose content depending on time and temperature.
Molecules 27 07783 g003
Figure 4. Contour plots of lignin content depending on time and temperature.
Figure 4. Contour plots of lignin content depending on time and temperature.
Molecules 27 07783 g004
Figure 5. UHPLC–ELSD chromatogram of the carbohydrate sample (1—xylose, 2—arabinose, 3—mannose, 4—glucose, 5—galactose, 6—HMF, 7—furfural).
Figure 5. UHPLC–ELSD chromatogram of the carbohydrate sample (1—xylose, 2—arabinose, 3—mannose, 4—glucose, 5—galactose, 6—HMF, 7—furfural).
Molecules 27 07783 g005
Figure 6. The proposed mechanism for transformation of hexoses into HMF.
Figure 6. The proposed mechanism for transformation of hexoses into HMF.
Molecules 27 07783 g006
Figure 7. Surface plot for xylose vs. temperature and time.
Figure 7. Surface plot for xylose vs. temperature and time.
Molecules 27 07783 g007
Figure 8. SEM images of (a) raw material, (b) raw material pretreated at 160 °C for 30 min, (c) raw material pretreated at 180 °C for 30 min, and (d) raw material pretreated at 200 °C for 30 min.
Figure 8. SEM images of (a) raw material, (b) raw material pretreated at 160 °C for 30 min, (c) raw material pretreated at 180 °C for 30 min, and (d) raw material pretreated at 200 °C for 30 min.
Molecules 27 07783 g008aMolecules 27 07783 g008b
Figure 9. FTIR images of (a) raw material, (b) cellulose standard, (c) glucose standard, (d) pretreated biomass at 160 °C for 30 min, (e) pretreated biomass at 180 °C for 30 min, and (f) pretreated biomass at 200 °C for 30 min.
Figure 9. FTIR images of (a) raw material, (b) cellulose standard, (c) glucose standard, (d) pretreated biomass at 160 °C for 30 min, (e) pretreated biomass at 180 °C for 30 min, and (f) pretreated biomass at 200 °C for 30 min.
Molecules 27 07783 g009
Figure 10. X-ray diffraction patterns of (a) raw material, (b) pretreated biomass at 160 °C for 30 min, (c) pretreated biomass at 180 °C for 30 min, and (d) pretreated biomass at 200 °C for 30 min.
Figure 10. X-ray diffraction patterns of (a) raw material, (b) pretreated biomass at 160 °C for 30 min, (c) pretreated biomass at 180 °C for 30 min, and (d) pretreated biomass at 200 °C for 30 min.
Molecules 27 07783 g010
Table 1. Chemical composition (% w/w) of the apple orchard waste (AOW).
Table 1. Chemical composition (% w/w) of the apple orchard waste (AOW).
AOW ComponentAmount (%/w/w)AOW ComponentAmount (%/w/w)
Lignocellulosic components Elemental analysis
Cellulose32.2 ± 0.07N0.78 ± 0.01
Hemicelluloses26.5 ± 0.05C46.7 ± 1.50
Insoluble lignin24.7 ± 0.07H5.79 ± 0.2
Soluble lignin0.52 ± 0.01S0.19 ± 0.01
Moisture6.96 ± 0.03Ash 2.04 ± 0.02
Extractables 2.5 ± 0.03
Table 2. Chemical compositions of the apple orchard waste after pretreatment at various temperatures. (Data represents mean ± standard deviation, n = 3).
Table 2. Chemical compositions of the apple orchard waste after pretreatment at various temperatures. (Data represents mean ± standard deviation, n = 3).
ParameterTemperature (°C)
160 °C–
15 min
180 °C–
15 min
200 °C–
15 min
160 °C–
30 min
180 °C–
30 min
200 °C–
30 min
160 °C–
45 min
180 °C–
45 min
200 °C–
45 min
Solid yield * 72. ± 2.163.1 ± 1.858.3 ± 2.369.2 ± 2.653.4 ± 1.551.7 ± 2.262.2 ± 2.351.2 ± 1.849.3 ± 1.6
Cellulose ** 37.2 ± 1.246.3 ± 1.644.2 ± 1.535.4 ± 1.445.3 ± 1.241.7 ± 1.337.2 ± 1.547.2 ± 1.245.3 ± 1.3
Hemicelluloses **19.6 ± 1.811.2 ± 0.099.1 ± 1.118.71 ± 1.210.1 ± 0.088.8 ± 0.075.4 ± 0.063.5 ± 0.042.2 ± 0.06
Lignin **33.0 ± 1.240.1 ± 1.546.2 ± 1.931.48 ± 2.138.1 ± 2.044.8 ± 2.328.3 ± 2.435.6 ± 2.640.2 ± 2.7
Solid compositions89.9 ± 2.397.6 ± 2.199.5 ± 2.285.6 ± 1.893.5 ± 1.795.2 ± 1.785.6 ± 1.493.5 ± 1.795.2 ± 1.8
* (% of raw material, dry biomass), ** (% of pretreated biomass, dry biomass).
Table 3. Analysis of variance for solid yield.
Table 3. Analysis of variance for solid yield.
SourceDFAdj SSAdj MSF-Valuep-Value
Model51637.60327.520110.020.000
 Linear21488.17744.085249.940.000
  Temp (°C)1993.09993.094333.590.000
  Time (min)1495.08495.076166.300.000
 Square2148.7874.38924.990.000
  Temp (°C) × Temp (°C)1144.39144.38748.500.000
  Time (min) × Time (min)14.394.3921.480.238
 Two-Way Interaction10.650.6530.220.644
  Temp (°C) × Time (min)10.650.6530.220.644
Error2162.522.977
 Lack of Fit336.0612.0198.180.001
 Pure Error1826.461.470
Total261700.12
DF—degree of freedom, SS—sums of squares, MS—mean sum of squares.
Table 4. Analysis of variance for cellulose content.
Table 4. Analysis of variance for cellulose content.
SourceDFAdj SSAdj MSF-Valuep-Value
Model5457.58291.51676.210.000
 Linear2212.770106.38588.590.000
  Temp (°C)1210.125210.125174.980.000
  Time (min)12.6452.6452.200.153
 Square2241.071120.536100.370.000
  Temp (°C) × Temp (°C)1216.400216.400180.200.000
  Time (min) × Time (min)124.67124.67120.540.000
 Two-Way Interaction13.7413.7413.120.092
  Temp (°C) × Time (min)13.7413.7413.120.092
Error2125.2181.201
 Lack of Fit36.0922.0311.910.164
 Pure Error1819.1271.063
Total26482.801
Table 5. Analysis of variance for hemicellulose content.
Table 5. Analysis of variance for hemicellulose content.
SourceDFAdj SSAdj MSF-Valuep-Value
Model5857.407171.481122.900.000
 Linear2663.231331.615237.670.000
  Temp (°C)1282.903282.903202.760.000
  Time (min)1380.328380.328272.590.000
 Square2146.33673.16852.440.000
  Temp (°C) × Temp (°C)143.88443.88431.450.000
  Time (min) × Time (min)1102.452102.45273.430.000
 Two-Way Interaction147.84047.84034.290.000
  Temp (°C) × Time (min)147.84047.84034.290.000
Error2129.3001.395
 Lack of Fit322.9437.64821.650.000
 Pure Error186.3580.353
Total26886.707
Table 6. Analysis of variance for lignin content.
Table 6. Analysis of variance for lignin content.
SourceDFAdj SSAdj MSF-Valuep-Value
Model5749.645149.929100.620.000
 Linear2725.549362.774243.460.000
  Temp (°C)1621.869621.869417.340.000
  Time (min)1103.680103.68069.580.000
 Square215.5957.7975.230.014
  Temp (°C) × Temp (°C)17.1147.1144.770.040
  Time (min) × Time (min)18.4818.4815.690.027
 Two-Way Interaction18.5018.5015.700.026
  Temp (°C) × Time (min)18.5018.5015.700.026
Error2131.2921.490
 Lack of Fit314.7254.9085.330.008
 Pure Error1816.5670.920
Total26780.936
Table 7. Model summary for RMS model.
Table 7. Model summary for RMS model.
s R2R2 (Adjusted)R2 (Predicted)
Solid yield1.7296.32%95.45%94.10%
Cellulose1.0994.78%93.55%91.29%
Hemicellulose1.1896.70%95.91%94.64%
Lignin1.2295.99%95.04%93.46%
Table 8. Prediction and optimization report obtained from multiple regression.
Table 8. Prediction and optimization report obtained from multiple regression.
Optimal SolutionsPredicted Value
(%)
Experimental Value (%) % of Variation Explained by the Modelp
Solid yield160 °C–15 min66.4265.52 ± 1.259.750.015
Cellulose 185.85 °C–45 min47.8148.23 ± 0.897.370.002
Hemicellulose160 °C–22.57 min18.0116.25 ± 0.388.810.008
Lignin200 °C–21.06 min45.8143.25 ± 1.197.91<0.001
Solid composition200 °C–45 min97.6496.35 ± 2.672.040.004
Table 9. Linearity, limit of detection (LOD), limit of quantification (LOQ), correlation coefficient (R2), and reproducibility of sugars.
Table 9. Linearity, limit of detection (LOD), limit of quantification (LOQ), correlation coefficient (R2), and reproducibility of sugars.
CompoundsRetention Time (min)Reproducibility (n = 10)
%CV
Regression Equation (y = ax + b)R2LOD
µg mL−1
LOQ
µg mL−1
Xylose5.6780.4y = 18.819x − 31.92880.99315.025.0
Arabinose6.1330.3y = 18.8039x − 20.98860.99215.025.0
Mannose7.0360.3y = 16.9589x − 61.12880.99815.025.0
Glucose7.2940.4y = 39.9770x − 192.00750.99715.025.0
Galactose7.6760.3y = 17.7075x − 65.32810.99815.025.0
Table 10. Statistical parameters of the calibration curve.
Table 10. Statistical parameters of the calibration curve.
CompoundsSySx0Recovery (%)VXOPG
Xylose172.239.1599.5 ± 4.27.092.5
Arabinose113.806.05107.2 ± 5.64.693.1
Mannose81.1884.7998.2 ± 4.83.714.6
Glucose214.535.37100.1 ± 6.24.155.5
Galactose78.7704.45104.2 ± 5.53.445.8
Sy—residual standard deviation, Sx0—standard error of the method, VXO—coefficient of variation of reproducibility (Sxo x 100/Xm), PG—the limits of working range ( s 1 2 s 6 2 ).
Table 11. Uncertainties of the analyzed sugars.
Table 11. Uncertainties of the analyzed sugars.
Purity
(%)
Uc rel
(mg L−1)
Uc
(mg L−1)
UE
(mg L−1)
Urel
(%)
Xylose99.00.10411.522.920.9
Arabinose98.00.0909.919.818.0
Mannose99.00.0859.318.616.9
Glucose99.50.0879.519.117.3
Galactose99.00.0889.719.517.7
Uc rel—combined standard uncertainties, U—combined uncertainty, UE—expanded uncertainty, Uerel—relative expanded uncertainty.
Table 12. The sugar (µg mL−1), furfural (µg mL−1), and HMF content (µg mL−1) in real samples (mean ± U (k = 2), n = 5 parallel samples).
Table 12. The sugar (µg mL−1), furfural (µg mL−1), and HMF content (µg mL−1) in real samples (mean ± U (k = 2), n = 5 parallel samples).
ParameterTemperature (°C)
160 °C–
15 min
180 °C–
15 min
200 °C–
15 min
160 °C–
30 min
180 °C–
30 min
200 °C–
30 min
160 °C–
45 min
180 °C–
45 min
200 °C–
45 min
Xylose581 ± 121601 ± 125587 ± 123784 ± 164889 ± 185.5770 ± 161685 ± 143708 ± 148681 ± 142
Arabinose789 ± 142815 ± 147797 ± 1441064 ± 1921207 ± 217.51045 ± 188930 ± 168961 ± 173925 ± 167
Mannose238 ± 40.3246 ± 41.7241 ± 40.7320 ± 54.2363 ± 61.5314 ± 53.2281 ± 47.5290 ± 49.1279 ± 47.2
Glucose66.1 ± 11.468.4 ± 11.866.8 ± 11.688.7 ± 15.3101 ± 17.487.1 ± 15.177.6 ± 13.480.2 ± 13.977.2 ± 13.3
Galactose156 ± 27.6161 ± 28.5158 ± 27.9210 ± 37.1239 ± 42.2207 ± 36.6184 ± 32.5190 ± 33.6183 ± 32.3
HMF22.1 ± 0.0729.3 ± 0.0625.3 ± 0.0425.6 ± 0.0530.2 ± 0.0839.5 ± 0.0532.0 ± 0.743.0 ± 0.650.0 ± 0.8
Furfural199 ± 1.5224 ± 0.8261 ± 0.9225 ± 0.21249 ± 0.34229 ± 1.1305 ± 1.3250 ± 1.8220 ± 1.2
Table 13. Analysis of variance for xylose.
Table 13. Analysis of variance for xylose.
SourceDFAdj SSAdj MSF-Valuep-Value
Model5242,79448,55999.200.000
 Linear238,88519,44239.720.000
  Temp11501500.310.585
  Time138,73538,73579.130.000
 Square2203,375101,688207.740.000
  Temp × Temp19815981520.050.000
  Time × Time1193,561193,561395.440.000
 Two-Way Interaction15335331.090.308
  Temp × Time15335331.090.308
Error2110,279489
 Lack of Fit3548118276.850.003
 Pure Error184799267
Total26253,073
Table 14. Model summary for RSM.
Table 14. Model summary for RSM.
R2R2 (Adjusted)R2 (Predicted)
Xylose 95.94%94.97%93.58%
Arabinose88.89%86.22%82.34%
Mannose87.54%84.57%79.29%
Glucose 72.55%66.02%57.19%
Galactose 89.13%86.54%82.41%
Table 15. Independent variables used for response surface studies.
Table 15. Independent variables used for response surface studies.
Variables Symbols Coded Levels
Low Factorial (−1)Center Point (0)High Factorial (+1)
Temperature (°C)X1160180200
Time (min)X2153045
Publisher’s Note: MDPI stays neutral with regard to jurisdictional claims in published maps and institutional affiliations.

Share and Cite

MDPI and ACS Style

Senila, L.; Scurtu, D.A.; Kovacs, E.; Levei, E.A.; Cadar, O.; Becze, A.; Varaticeanu, C. High-Pressure Supercritical CO2 Pretreatment of Apple Orchard Waste for Carbohydrates Production Using Response Surface Methodology and Method Uncertainty Evaluation. Molecules 2022, 27, 7783. https://doi.org/10.3390/molecules27227783

AMA Style

Senila L, Scurtu DA, Kovacs E, Levei EA, Cadar O, Becze A, Varaticeanu C. High-Pressure Supercritical CO2 Pretreatment of Apple Orchard Waste for Carbohydrates Production Using Response Surface Methodology and Method Uncertainty Evaluation. Molecules. 2022; 27(22):7783. https://doi.org/10.3390/molecules27227783

Chicago/Turabian Style

Senila, Lacrimioara, Daniela Alexandra Scurtu, Eniko Kovacs, Erika Andrea Levei, Oana Cadar, Anca Becze, and Cerasel Varaticeanu. 2022. "High-Pressure Supercritical CO2 Pretreatment of Apple Orchard Waste for Carbohydrates Production Using Response Surface Methodology and Method Uncertainty Evaluation" Molecules 27, no. 22: 7783. https://doi.org/10.3390/molecules27227783

Article Metrics

Back to TopTop