The Catalytic Performance of Nanorod Nickel Catalyst in the Hydrolysis of Lithium Borohydride and Dimethylamine Borane
Next Article in Special Issue
Sonocatalytic Degradation of Chrysoidine R Dye Using Ultrasonically Synthesized NiFe2O4 Catalyst
Previous Article in Journal
AAO-Assisted Nanoporous Platinum Films for Hydrogen Sensor Application
Previous Article in Special Issue
Synthesis of Novel Zn3V2O8/Ag Nanocomposite for Efficient Photocatalytic Hydrogen Production
 
 
Font Type:
Arial Georgia Verdana
Font Size:
Aa Aa Aa
Line Spacing:
Column Width:
Background:
Article

A Comparison of Different Reagents Applicable for Destroying Halogenated Anionic Textile Dye Mordant Blue 9 in Polluted Aqueous Streams

by
Barbora Kamenická
and
Tomáš Weidlich
*
Chemical Technology Group, Institute of Environmental and Chemical Engineering, Faculty of Chemical Technology, University of Pardubice, Studentska 573, 532 10 Pardubice, Czech Republic
*
Author to whom correspondence should be addressed.
Catalysts 2023, 13(3), 460; https://doi.org/10.3390/catal13030460
Submission received: 6 January 2023 / Revised: 27 January 2023 / Accepted: 31 January 2023 / Published: 22 February 2023
(This article belongs to the Special Issue Advanced Oxidation Catalysts)

Abstract

:
This article aimed to compare the degradation efficiencies of different reactants applicable for the oxidative or reductive degradation of a chlorinated anionic azo dye, Mordant Blue 9 (MB9). In this article, the broadly applied Fenton oxidation process was optimized for the oxidative treatment of MB9, and the obtained results were compared with other innovative chemical reduction methods. In the reductive degradation of MB9, we compared the efficiencies of different reductive agents such as Fe0 (ZVI), Al0, the Raney Al-Ni alloy, NaBH4, NaBH4/Na2S2O5, and other combinations of these reductants. The reductive methods aimed to reduce the azo bond together with the bound chlorine in the structure of MB9. The dechlorination of MB9 produces non-chlorinated aminophenols, which are more easily biodegradable in wastewater treatment plants (WWTPs) compared to their corresponding chlorinated aromatic compounds. The efficiencies of both the oxidative and reductive degradation processes were monitored by visible spectroscopy and determined based on the chemical oxygen demand (COD). The hydrodechlorination of MB9 to non-chlorinated products was expressed using the measurement of adsorbable organically bound halogens (AOXs) and controlled by LC–MS analyses. Optimally, 28 mol of H2SO4, 120 mol of H2O2, and 4 mol of FeSO4 should be applied per one mol of dissolved MB9 dye for a practically complete oxidative degradation after 20 h of action. On the other hand, the application of the Al-Ni alloy/NaOH (100 mol of Al in the Al-Ni alloy + 100 mol of NaOH per one mol of MB9) proceeded smoothly and seven-times faster than the Fenton reaction, consumed similar quantities of reagents, and produced dechlorinated aminophenols. The cost of the Al-Ni alloy/NaOH-based method could be decreased significantly by applying a pretreatment with Al0/NaOH and a subsequent hydrodechlorination using smaller Al-Ni alloy doses. The homogeneous reduction accompanied by HDC using in situ produced Na2S2O4 (by the action of NaBH4/Na2S2O5) was an effective, rapid, and simple treatment method. This reductive system consumed quantities of reagents that are almost twice as low (66 mol of NaBH4 + 66 mol of Na2S2O5 + 18 mol of H2SO4 per one mol of MB9) in comparison with the other oxidative/reductive systems and allowed the effective and fast degradation of MB9 accompanied by the effective removal of AOX. A comparison of the oxidative and reductive methods for chlorinated acid azo dye MB9 degradation showed that an innovative combination of reduction methods offers a smooth, simple, and efficient degradation and hydrodehalogenation of chlorinated textile MB9 dye.

Graphical Abstract

1. Introduction

Azo dyes are the most important synthetic colorants and have been used for a wide spectrum of textile dyeing [1,2]. Acid dyes soluble in aqueous solutions are usually applied for dyeing natural fibers [3,4]. Mordant dyes derived from acid dyes have been widely used for the coloration of textile fibers such as wool, silk, polyester, cotton, and some modified cellulose fibers [5,6,7,8]. One example of the mentioned mordant azo dyes is the acid dye Mordant Blue 9 (MB9, Figure 1). However, the effective treatment of dye baths and wastewater from dye production and utilization before they are released to the environment has received significant attention because of their potential toxic effects based on the fact that Mordant dyes are difficult to degrade [9].
On average, the annual production of dyes exceeds 7 × 105 tons. However, in the textile industry, typically about 10% of the used dyes are discharged, with the effluent creating both environmental and economic issues due to the limited biodegradability of azo dyes, especially halogenated ones [10]. The occurrence of especially halogenated non-biodegradable azo dyes in wastewater not only deteriorates water aesthetically due to its coloration but also increases its chemical oxygen demand (COD) and adsorbable organic halogen content (AOX) [11].
Various removal methods have been developed to remove the dyes produced during the dyeing of textile fabrics from wastewater. However, the effective destruction of non-biodegradable azo dyes in effluents does not only comprise decolorization [12,13,14,15,16,17]. The practical removal of spent dyes in wastewater streams should be accompanied by the formation of easily biodegradable products or by the complete mineralization of the original dye to CO2, H2O, nitrate or N2, sulphate, etc. [16,17].
Fenton-based advanced oxidation processes (AOPs) are among the most effective processes because of their relative ease of operation, low-cost facilities, and high removal efficiency [18].
Fenton oxidation degrades organic pollutants by applying hydroxyl radicals (HO∙), which are generated from a hydrogen peroxide (H2O2) + ferrous sulfate reaction in an acidic medium [19]. However, the common application of Fenton processes is limited by several limitations, such as acidic pH conditions, iron-based sludge generation, and the large consumption of hydrogen peroxide [20].
The large consumption of H2O2 in Fenton oxidation is caused by the high reactivity (low stability) of the produced OH∙ radicals together with the easier degradability of the organic oxidation products compared to the starting pollutant [18]. In the case of chemical oxidation, a complete mineralization is typically necessary for the removal of toxic and non-biodegradable halogenated organic by-products such as AOX [13].
Some improvements in the utilization of the oxidant used in chemical oxidation processes provides the substitution of hydrogen peroxide with persulfate (S2O82−) [18].
The formation of the sulfate radical ∙SO4 from alkali metal persulfate is commonly catalyzed by the action of transition metal ions such as Fe2+, Co2+, etc. The sulfate radical works as a strong oxidant possessing a higher redox potential and an even higher span of its half-life stability compared with hydroxyl radicals [21,22,23,24,25,26,27].
However, the higher price of persulfate (800–1160 USD/t of Na2S2O8 [28]) compared to hydrogen peroxide (350–450 USD/t of H2O2 [29]) and the secondary contamination of treated water with inorganic sulphates are the limitations of persulfate-based AOPs.
Compared with chemical oxidation, the chemical reduction method enables more selective reductive cleavage of azo or other simply reducible bonds (NO2, etc.) [30]. Applying appropriate reductants, it facilitates the effective hydrodehalogenation of carbon-halogen bonds that occur in many synthetic dyes (the reductive removal of AOX-producing inorganic halides) [31].
Several papers [32,33,34,35] have described the reductive degradation of azo dyes using zero-valent iron (Fe0 or ZVI) or nano ZVI. However, ZVI is not able to effectively reduce carbon–halogen bonds in halogenated aromatic compounds [33].
As we recently published, the Raney Al-Ni alloy is an excellent hydrodechlorination (HDC) agent [30,31]. Hydrodehalogenation using Al-based alloys is based on dissolving aluminium in the sodium hydroxide solution. Hydrogen is thus produced and adsorbed on the catalytically acting nickel surface which subsequently converts chlorinated organic compounds into non-halogenated products, which are easily biodegradable [36].
The other reduction method for effective azo dye degradation mentioned in the literature is based on sodium borohydride (NaBH4) reduction or on sodium dithionite (Na2S2O4) produced in situ by the co-action of NaBH4 and Na2S2O5 [37].
With the emphasis on MB9, only a few articles were focused on the removal of this mentioned dye [13,18,38,39,40,41]. The previous article of our research group [13] reported the separation of MB9 using ionic liquids. As we presented in this article, the isolation method of MB9 using ionic liquids provides the effective removal of the tested dye [13]. The separation of MB9 by adsorption was consequently studied in several publications [38,39,40]. As shown by Singh et al., the microbial degradation of MB9 dye enables the effective discoloration of aqueous solutions contaminated with this dye. The level of MB9 HDC is low [41].
Only one article [18] focused on the oxidative degradation of MB9 using the Fenton-activated persulfate system. Pervez et al. reported the effective degradation of MB9 using the above-mentioned method expressed with discoloration and TOC removal efficiency. However, the authors did not control the possible dehalogenation of MB9 [18].
The aim of this article is to compare the effectiveness of chlorinated anionic azo dye Mordant Blue 9 (Figure 1) degradation in an aqueous solution using oxidation or reduction techniques. We compare the broadly applied Fenton reaction with innovative reduction methods.

2. Results and Discussion

2.1. Chemical Oxidation of MB9 Using H2O2

All the experiments were performed using a model aqueous solution of MB9 simulated industrial (real) wastewater from the production of acid azo dyes [42]. The applied final concentration of MB9 in reaction mixtures was 0.25 mmol/L (125 mg/L).
The initial experiments were conducted using an excess of hydrogen peroxide with overnight vigorous stirring (20 h) for the possible mineralization of MB9 dye according to Equation (1):
C16H9ClN2O8S2Na2 + 35 H2O2 → 16 CO2 + 38 H2O + 1 HCl + N2 + 2 NaHSO4
In experiments of MB9 oxidation using H2O2, we demonstrated the degradation of MB9 using absorbance and discoloration efficiency measurements. The CODCr was applied to determine the removal of organic compounds after oxidation quenching by the addition of 0.1 g MnO2 which causes the decomposition of residual H2O2 (see the Materials and Methods section). Due to the study of chlorinated compound MB9 degradation, AOX was then determined, which expressed the content of chlorinated compounds in samples before and after degradation.
The fragmentation products of MB9 oxidation were not utilized due to complex oxidation pathways. As shown in Equation (1), theoretically at least 35 mol of H2O2 is necessary for the complete mineralization of 1 mol of MB9.
Figure 2 shows that using 20 mol of H2O2 per mol of MB9, the MB9 dye molecule was destroyed with 92% efficiency after 20 h of action according to the colour removal (measured as absorbance at absorption maximum in the visible spectrum). According to the COD determination, however, less than 10% of oxidizable organic compounds were mineralized under these reaction conditions (using 1 mmol of H2O2 per 0.05 mmol of MB9). The gradual increase in hydrogen peroxide dosage only caused a slow increase in COD removal. Using a 40-fold molar excess of H2O2 above the MB9 dye, only around 10% of COD (and around 93% of MB9) was removed, even after 20 h of action. This observation is in apparent contradiction with the theoretical consumption of H2O2 necessary for the complete mineralization of MB9 to inorganic products (Equation (1)). Even when 200 mol of H2O2 per mol of MB9 was used, the COD value decreased to only 40% of the initial quantity (10 mmol of H2O2 used per 0.05 mmol of MB9, as shown in Figure 2).
In the subsequent reaction experiments, the ferrous sulphate was added to the acidified mixture of MB9 (2 mL of 16% H2SO4 was added to 200 mL of aqueous MB9 solution containing 0.05 mmol of MB9, and the pH was adjusted in pH interval 2–2.5) and stirred with an appropriate quantity of H2O2 with the aim of utilizing the oxidation ability of OH∙ radical produced from the Fenton reaction (Equation (2)):
Fe2+ + H2O2 → OH∙ + Fe3+ + OH
The applied low pH value was used with the aim of minimizing the possibility of iron (hydr)oxide precipitation during the Fenton oxidation process. As Kremer [43] reported, the optimum pH can also be lower than 3 for an efficient Fenton reaction. The studied dependence of discoloration efficiency/COD removal on the pH value is illustrated by Figure S1 in the Supplementary Materials. It was demonstrated that that there are no significant changes in discoloration efficiencies/COD removal in the range of pH values 2–4. Based on these reasons, the pH value was adjusted to pH = 2–2.5. Our experiments were therefore focused on the adjustment of the optimum dosage of H2SO4 for ensuring the acidic environment and efficient oxidation of MB9.
The addition of 2 mL of 16% H2SO4 per 200 mL of aqueous 0.25 mM MB9 solution (with a pH value of 2–2.5 and an efficient Fenton oxidation, as shown in Figure 3).
As shown in Figure 3, the Fenton oxidation initialized by the addition of FeSO4 to the acidified MB9 solution significantly increased the COD removal process (compared with the action of sole H2O2). In the case of a 40-fold molar excess of H2O2 towards MB9, the ferrous sulphate addition enabled the 60% removal of oxidizable matter. By using 6 mmol of H2O2 and 0.06 mmol of FeSO4 per 0.05 mmol of MB9 (molar ratio [Fe2+]/[H2O2]/[MB9] = 1.2:120:1), the removal of MB9 was practically quantitative and subsequently around 82% of oxidizable matter was removed by Fenton oxidation (according to the COD removal efficiency). Similar [Fe2+]/[H2O2] ratios were reported as most effective by Gulkaya et al. for spent dye bath oxidative treatment [19]. Without FeSO4, the COD removal was low (with a COD removal efficiency below 20%).
For a subsequent biological wastewater treatment plant (WWTP), AOX removal during the chemical oxidation of recalcitrant chemicals is most important, especially due to the biocidal effect of many chlorinated compounds such as halogenated phenols [44,45].
The MB9 removal efficiency caused by Fenton oxidation was compared with AOX removal efficiency using an excess of the Fenton reagent in an optimized molar ratio 1 mol of FeSO4 per 100 mol of H2O2. As is illustrated in Figure 4, both AOXs and decolorization efficiencies were quite similar (88% of MB9 removal and 86% of AOX removal) and high enough using the molar ratio [Fe2+]/[H2O2]/[MB9] = 0.2:20:1, even after 4 h of action.
We observed that the prolonged reaction time of Fenton oxidation is an important parameter for the maximization of AOX and COD removal (Figure 5 below). Due to this reason reaction time, 20 h was applied in the subsequent experiments.
The effect of different molar ratios [Fe2+]/[H2O2]/[MB9] = 1–4:10–120:1 is illustrated in Figure 5 and Figure 6. Comparing the relationship between the molar ratios of FeSO4 and H2O2, [Fe2+]/[H2O2] = 1:20–30 seems to be more effective. It is evident that for the fairly complete removal of MB9 and AOX, at least 120 mol of H2O2, together with 4 mol of FeSO4 per mol of MB9, should be used (Figure 6 and Figure 7). This means that the actual minimal excess of H2O2 is more than 3–3.4 times higher compared to the theoretical consumption of H2O2 for the complete mineralization of MB9 (see Equation (1)).
Despite the high discoloration efficiency of MB9 using Fenton reaction after 4 h (see Figure 7), the removal of COD and AOX did not amount to satisfactory results, as shown in Figure 6. Therefore, the prolonged reaction time (20 h) in combination with high dosages of H2O2/Fe2+ was proven to be necessary for the effective degradation of MB9 (including AOX and COD removal).
Under described conditions, however, the [Fe2+]/[H2O2] ratio seems to be far from optimal [46], likely accompanied by a high consumption of H2O2. The real excess of H2O2 was more than 3–3.5-times higher compared to the theoretical consumption (see Equation (1)).
Due to the reasons mentioned above, optimization experiments were performed with the aim of rationalizing the dosage of components of the Fenton reagent.
Compared with the persulfate-based method [18], the required excess of H2O2 for the practically complete removal of AOX and COD seems to be high. However, the published persulfate method only determined residual TOC and MB9 removal, not a concentration of hardly biodegradable and toxic AOXs. For 95% discoloration, a similar 10-fold molar excess of H2O2 and an equimolar quantity of FeSO4 toward MB9 should be used (Figure 5, second column from the left).
Finally, it is evident that the subsequent neutralization of the reaction mixture after Fenton oxidation increases the additional removal of MB9 (almost a 20% increase in the COD removal efficiency) caused by the coagulation of iron (hydr)oxides, as shown in the Supplementary Materials, Table S1. By neutralizing the acidic reaction mixture, in contrast, the produced solid by-product (iron (hydr)oxides containing slurry) is potentially contaminated with adsorbed oxidation (chlorinated) products. This slurry is categorized as a dangerous waste and must be disposed in a safe manner [47].

2.2. The Chemical Reduction of MB9

Compared with chemical oxidation, the chemical reduction of pollutants was described as more selective [30,31]. A higher selectivity is joined with a lower consumption of reagents.
In the first set of experiments, iron turnings (ZVI) were used for the reductive degradation of MB9.
The obtained results are illustrated in Figure 8. ZVI is a strong reducing agent, and moreover ZVI is easily produced and inexpensive [32]. It has already been rendered to be effective in the reductive degradation of selected chlorinated organic derivatives [48]. In some studies [33,34], methods of dye reduction using micro or nano iron have been described.
Even using a 10-fold molar excess of ZVI, 97% of MB9 was removed. The AOX removal efficiency, however, was low (25.9%). This corresponds with the known fact that ZVI is not a very effective dechlorination agent in the case of chlorinated aromatic compounds. In the case of a 150-fold molar excess of ZVI, only a 35.2% AOX removal efficiency was observed (together with a 99.5% MB9 removal efficiency).
Apart from ZVI, metallic aluminum (granules, powder, or foil) was tested for the reductive degradation of MB9 dye. Aluminum was reported to be more effective in wastewater treatment compared with ZVI [35]. Figure 9 illustrates differences in Al0-based reduction efficiencies using diluted sulfuric acid. In addition to Al0, the Raney Al-Ni alloy, known to be very effective reductant, was used [30,31]. The obtained degradation efficiencies were slightly worse using Al0 compared with Fe0.
It is well known that Al0 is a powerful reductant, especially in diluted alkali metal hydroxide solutions [35]. For this reason, alkaline conditions were used for subsequent experiments. The obtained results are presented in Figure 10.
When using Al powder in particular, both MB9 and AOX removals were higher compared with ZVI/H2SO4 or Al0/H2SO4 actions. In addition, the used Al granules were similarly active as Al foil, although both above-mentioned forms of Al were less active compared with Al powder. In the case of the used Al granules, a low specific surface seems to be the reason for the low reduction activity. In addition, the kinetic comparison indicates that the reaction rate of Al0/NaOH was higher (Figure 11).
Due to our excellent experience with the hydrodehalogenation activity of Al-Ni alloys [30,31], we tried to use a mixture of Ni powder together with Al0 (Figure 10) and Raney Al-Ni alloys for MB9 reductive treatment (Figure 12). After the addition of Ni powder, both the MB9 and AOX removal efficiencies increased in comparison with the action of Al0 alone. Using the Raney Al-Ni alloy, however, the HDC of MB9 reduction products was much higher compared with the action of a mixture of Al0 and Ni0 powders.
In addition, by using the Raney Al-Ni alloy instead of Al0 + Ni0 powders, the removal of AOX (hydrodechlorination, HDC) was very effective (Figure 12) [30,31]. HDC was completed after 3 h of Al-Ni alloy/NaOH action. In comparison with the Fenton reaction, HDC using Al-Ni alloy/NaOH processed almost seven times faster in the degradation of MB9. The proposed reaction pathway for the reductive treatment of MB9 using Al0 + Ni0 or Al/Ni alloys is depicted in Scheme 1.
A combination of the rapid azo bond reduction of the MB9 structure using cheaper Al0 powder (pretreatment) and subsequently HDC using the Al-Ni alloy (see Scheme 1) serves as a simple cost-effective application in the degradation of non-biodegradable chlorinated dye in aqueous streams. Non-chlorinated products based on the reduction/HDC of this promising reductive method were proved using the LC-MS method. As indicated by LC-MS analysis (see Supplementary Material, Figure S2), the HDC of MB9 using Al-Ni (Figure 12, first column from the left, 3 h of action) proceeded smoothly according to the HDC reaction depicted in Scheme 1.
The starting Raney Al-Ni alloy and its reaction products were studied by X-ray powder diffraction in our earlier work [30]. The changes in surface morphology were also documented by SEM [30]. As we published earlier, the starting Raney Al-Ni alloy contained 41% Ni2Al3, 57% NiAl3, and 2% aluminum. Briefly, after the beginning of the reaction (after 30 min of HDC of chloroaromates (using 0.27 g of Al-Ni/1 mmol Ar-Cl + 50 mmol of NaOH), the original Raney Al-Ni alloy changed slightly, the pure aluminum disappeared, and the NiAl3 alloy quantity decreased (34% NiAl3 and 66% Ni2Al3). After 60 min of the reaction, the NiAl3 diffraction lines disappeared completely, and the isolated solid part only contained Ni2Al3. At the end of the HDC reaction, apart from the rest of Ni2Al3 (18%), the isolated solid mainly contained Ni0.92Al0.08 alloy (61%) and pure metallic nickel (10%), together with a low quantity of bunsenite (2% NiO) [30].
In addition, after the HDC, the produced nickel sludge was simply removable by sedimentation and/or filtration. The deactivated Ni catalyst can be regenerated and recycled with several benefits [49].
The dissolved aluminum in the alkaline reaction mixture after HDC can be utilized for the subsequent sorption of HDC products via the coagulation and flocculation of Al(OH)3 produced by alkaline aqueous phase neutralization after the HDC procedure [30,31,49,50,51].
The above-mentioned coagulation also increased the COD removal efficiency by up to 15% (see the Supplementary Materials, Table S1).
The HDC of MB9 using Al-Ni therefore effectively removed AOX, and, subsequently, the neutralization of the reaction mixture, accompanied by coagulation, facilitated additional COD removal. In contrast with the Fenton reaction, this slurry after coagulation contains more biodegradable (non-chlorinated) HDC products and it can be used as an additive for cement production.
In the above-mentioned Al-based MB9 removal methods, the sorption of MB9 on the surface of Al-based reductive agents could play an important role. The sorption experiments were performed to compare the sorption effect on MB9 removal using different sources of Al0.
A comparison of sorption efficiencies is illustrated in Figure 13 (the contact time was 3 h). The highest removal efficiency of MB9 was obtained with Al0 powder (MB9 65.8%) or Al0 foil (59.5%). A similar removal efficiency was achieved by the Raney Al-Ni alloy (60%), as shown in Figure 13. Al0 granules were not very efficient for MB9 sorption, possibly due to the low specific surface area of Al granules.
In addition, the calculated sorption parameter—adsorption capacity q (mg/kg)—demonstrated that the sorption capacities of Al powder and Al foil for MB9 dye were 65.8 mg/kg and 59.5 mg/kg, respectively. In contrast, the adsorption capacity of the Raney Al-Ni alloy was only 30 mg/kg.
Despite this fact, the results indicate that MB9 is selectively adsorbed, especially on powders of aluminum or Raney Al-Ni alloys or Al foil. From the above-mentioned results, it can be deduced that the main drawback of the used Al foil in the reduction process is its very rapid dissolution (consumption) under the used reaction conditions (over a few minutes, as was observed), which prevents the effective MB9 reductive removal.
A comparison of decolorization rates based on the application of Al0 in alkaline and acidic reaction conditions is illustrated in Figure 14. It is evident that the removal of MB9 dye is the most rapid when the Al0-based reduction process is used in aqueous NaOH. The reaction rates of the Fenton oxidation and Al0-based reduction of aqueous H2SO4 were quite similar.
Another reduction method for effective azo dye degradation mentioned in the literature is based on sodium borohydride (NaBH4) or sodium dithionite (Na2S2O4, see reactions 3 and 4) produced in situ by the reaction of NaBH4 with Na2S2O5 [37] (Scheme 2). It was verified that sodium borohydride caused efficient MB9 reduction when applied alone; however, the AOX removal was sluggish (Figure 15).
S2O52− + H2O → 2 HSO3
BH4 + 8 HSO3 + H+ → 4 S2O42− + B(OH)3 + 5 H2O
When applying a combination of cheap Na2S2O5 accompanied by the subsequent addition of NaBH4, both MB9 and AOX were removed very effectively (Figure 15). The proposed reaction scheme of MB9 reductive degradation using NaBH4/Na2S2O5 is illustrated in Scheme 2. As indicated by LC-MS analysis (see Supplementary Material, Figure S3), a smooth reduction of MB9 is depicted in Scheme 2.
Table 1 shows a comparison of the above-described results of the oxidation and reduction of MB9 (calculated per one mol of tested dye for the demonstration of practical application). The reaction rates of the tested reduction processes are compared in Figure 16. It is evident that the homogeneous reduction using NaBH4/Na2S2O5 is the most rapid process weighted by decolorization. A comparison of reagents consumption and degradation efficiencies in performed optimized experiments is depicted in Figure 17. The pretreatment of MB9 solutions using Al0/NaOH and subsequently HDC with Al-Ni/NaOH also facilitates the effective and smooth removal of MB9 dye.
In summary, the Fenton reaction is cheaper than other tested reductive systems (see Supplementary Materials, Table S2) due to the low cost of hydrogen peroxide. The reaction rate, however, is slow, even when using an excess of H2O2 that is more than 3.5 times higher than that using the theoretical consumption. On the other hand, for the practical rapid removal of AOX necessary for scale-up, reductive systems such as NaBH4/Na2S2O5 or a combination of Al0/Al-Ni alloys are more utilizable.
The above-mentioned combination of NaBH4/Na2S2O5 or Al0/Al-Ni alloys provides an increase in the removal of MB9 from model wastewater. These methods also offer a decrease in price compared with less efficient/more expensive reductions using NaBH4 or Al-Ni alloy alone (see the Supplementary Materials, Table S2).
Moreover, HDC using Al-Ni alloys proceeds smoothly in a few hours in contrast with HDC using the Fenton reaction (reaction time for effective MB9 removal 20 h, as shown in Table 1). The lower reaction time of the proposed reductive process saves energy and further decreases economic costs. In addition, the application of the Al-Ni alloy enables the recycling of produced Ni-slurry [49,50,51]. This recycling of used Al-Ni alloys also potentially decreases the price of this effective HDC method.

3. Materials and Methods

3.1. Reagents and Materials

The acidic azo dye Mordant Blue 9 (MB9) was purchased from commercial sources in a defined purity 50% of MB9 (Sigma Aldrich Co., Prague, Czech Republic). Sigma-Aldrich does not provide the exact composition of the other ingredients. It can be assumed, however, that other ingredients are inorganic salts from dye manufacturing [6].
H2O2 (30%) and FeSO4.7H2O (p.a. quality) were obtained from Lach-Ner Co., Neratovice, Czech Republic. The Raney Al-Ni alloy, NaBH4, and Na2S2O5 were supplied from Sigma Aldrich Co., Prague, Czech Republic. The powdered Al0 (Labo MS Co., Prague, Czech Republic), granulated Al (Lachema Co., Brno, Czech Republic), Al foil, powdered Ni (Alfa Aesar, Heysham, Lancashire, UK), and zero-valent Fe0 (ZVI, local supplier Synthesia Co., Pardubice, Czech Republic) were purchased in purity higher than 95%. Additional chemicals (H2SO4, NaOH and MnO2) in p.a. quality were obtained from Lach-Ner Co., Neratovice, Czech Republic. Finally, all the aqueous solutions were prepared from demineralized water.

3.2. Oxidative and Reductive Degradation of MB9 Procedures

The comparative degradation experiments were performed in a 250 mL round-bottomed flasks equipped with magnetic stirring on Starfish equipment (Radleys Discovery Technologies, Saffron Walden, UK), installed on a magnetic stirrer Heidolph Heistandard for parallel reactions. The reaction flasks were closed by a tube filled with granulated charcoal. After the appropriate time period of stirring, the reaction mixtures were filtered and analyzed.
In the case of the oxidative degradation of MB9 using hydrogen peroxide, all the samples were mixed before filtration with 0.1 g of MnO2 used as the catalyst for the rapid decomposition of unreacted H2O2. The final measurement of residual H2O2 in the reaction mixtures was not required and the interferences of COD determination were negligible (unreacted H2O2 significantly increased the COD value, as verified). For the Fenton reaction, the pH values of reaction mixtures were modified using the addition of 10 mL of 16% H2SO4 per liter of 0.5 mM aqueous MB9 solution (2 mL of 16% H2SO4 per 200 mL of H2O containing 0.05 mmol of MB9). The pH values were measured and/or controlled by a contact pH meter Orio Star 10 (Thermo Fisher Scientific, Pardubice, Czech Republic).
In the case of the ZVI application, due to the limitation of the magnetic stirring influence, the reaction mixtures were intensively stirred. Thus, the sufficient contact of ZVI with the aqueous solutions of MB9 was ensured.

3.3. Chemical Analysis

A Hach DR2800 (Austria) VIS spectrophotometer was employed for the absorbance measurements using 1 cm glass cuvettes. The concentrations of MB9 were determined by measuring at a wavelength 516 nm. Analyses of the COD were carried out in accordance with the ISO EN 9562 standard and aqueous solutions were determined using the Hach Lange cuvette test using the Hach DR2800 (Austria) VIS spectrometer. The AOXs were analyzed according to the European ISO 9562 standard using the Multi X 2500 analyzer (Analytic Jena GmbH., Jena, Germany).
The discoloration of MB9 solutions was calculated according to Equation (5):
D E = ( 1 A A 0 ) × 100
where DE is the discoloration efficiency of MB9 aqueous solution (%), A is the measured absorbance after the degradation process, and A0 is the initial absorbance of MB9 solution.
The removal efficiency (%) of COD or AOX from the model aqueous solutions of MB9 was evaluated by Equation (6):
R E = ( 1 c c 0 ) × 100
where RE is removal efficiency of AOX or COD (%), c is the concentration of AOX or COD in the solution after the degradation process (mg/L), and c 0 is the initial concentration of AOX or COD in the MB9 solution before the degradation process (mg/L).
The reduction products after the reductive degradation of MB9 were detected using the LC-MS technique with additional UV detection. The water samples were properly diluted and 2 μL of the diluted sample was injected in the Hypersil Gold C4 column (100 × 3 mm). The LC separation of the detected compounds was performed in a LC-MSD TRAP XCT Plus system (Agilent Technologies, Santa Clara, CA, USA) and was carried out with a gradient program using (A) 5 mM CH2COONH2, (B) 95% CH3COONH4, and (C) acetonitrile at a flow rate of 0.5 mL/min and at temperature of 40 °C. The detected compounds were completely separated under the established gradient program in 40 min. The UV detection was carried out at a wavelength 254 nm. The LC system was connected to an Agilent 6490 Triple Q MS with an electrospray interface (ESI) and was operated in both positive and negative ionization mode, using the above-described gradient program in both cases. The MS settings were as follows: a drying gas temperature of 350 °C; a drying gas of 10 L/min; ion source gas of 50 psi; and a mass range of 50–1200 Da. Nitrogen was used as the nebulizer gas, curtain gas, and collision gas.

4. Conclusions

This paper aims to compare the efficiency of common Fenton oxidation together with innovative chemical reduction of chlorinated anionic azo dye Mordant Blue 9 to simply biodegradable nonchlorinated products.
The classic Fenton oxidation is broadly used and is a frequently evaluated treatment method using cheap and low toxic reagents, such as hydrogen peroxide and ferrous sulphate. These reagents cause the negligible secondary contamination of treated and subsequently neutralized water free of insoluble impurities such as iron (hydr)oxides.
We demonstrated that an appropriate excess of hydrogen peroxide (120 mol), H2SO4 (28 mol), and FeSO4 (4 mol) is able to destroy chlorinated acid azo dye Mordant Blue 9 to non-chlorinated by-products with the subsequent removal of oxidizable organic compounds after 20 h of action. By neutralizing the acidic reaction mixture, the produced solid by-product, including iron (hydr)oxides containing slurry, is potentially contaminated with adsorbed oxidation products. This slurry is categorized as dangerous waste and must be disposed in a safe manner. In addition, the large consumption of reagents could disfavor the Fenton oxidation for potential large-scale application.
The tested reductive wastewater treatment methods are less common compared with chemical oxidation. Using appropriate reduction agents, the chemical reduction serves as a simple and economically attractive method for the destruction of a hardly biodegradable compound, such as chlorinated azo dye MB9, to non-chlorinated by-products suitable for subsequent biodegradation in common wastewater treatment plants.
Both ZVI/H2SO4 and Al0/H2SO4 are effective azo reduction bonds, but poor HDC agents. The same inconvenience was observed in the case of Al0/NaOH action. In contrast, the heterogeneous reductant Raney Al-Ni alloy in NaOH and the homogeneous reductant NaBH4/Na2S2O5 alloy are very effective for both azo bond reduction and subsequent HDC.
There is still uncertainty around (i) the minimal quantity and the price of effective reductants applicable for both the azo bond reduction and effective HDC of produced chlorinated aminophenol- and aminonaphtol-based sulphonic acids and (ii) the accompanying treatment of produced by-products descended from used reductants/HDC agents.
From the consumption of the reagents point of view, the homogeneous reduction accompanied by HDC using Na2S2O4 produced in situ (by the action of NaBH4/Na2S2O5) is the most effective, rapid, and simple destruction method.
An innovative heterogeneous reduction combining pretreatment with Al0/NaOH with the subsequent addition of effective HDC agents (Raney Al-Ni alloy/NaOH) is more exacting. In the case of the used Al-Ni alloy, the recycling of produced Ni-slurry was demonstrated earlier with the aim of obtaining an effective hydrodehalogenation agent.

Supplementary Materials

The following supporting information can be downloaded at: https://www.mdpi.com/article/10.3390/catal13030460/s1, Figure S1: The dependence of discoloration efficiency/COD removal on the pH value for the Fenton reaction using 6 mmol of H2O2 + 0.2 mmol of FeSO4 per 0.05 mmol of MB9 in 200 mL of H2O (reaction time 20 h). Figure S2: LC chromatogram of LC-MS analysis of the reaction mixture obtained after the reductive degradation of MB9 using Al-Ni/NaOH. Figure S3a: LC chromatogram of LC-MS analysis of reaction mixture obtained after the reductive degradation of MB9 using NaBH4/Na2S2O5. Figure S3b: Qualitative LC-MS analysis of the reaction mixture obtained after the reductive degradation of MB9 using NaBH4/Na2S2O5. Figure S3c: Mass spectrums (EI, 70 eV) of analyzed components. Table S1: The effect of subsequently coagulation on Fenton reaction and reduction/HDC using the Al-Ni alloy. Table S2: A comparison of economic viability of MB9 removal using different oxidative/reductive agents [52,53,54,55,56,57,58,59,60,61,62].

Author Contributions

Conceptualization, T.W.; methodology, T.W.; software, B.K.; validation, B.K.; formal analysis, B.K.; investigation, B.K. and T.W.; resources, T.W.; data curation, B.K.; writing—original draft preparation, T.W.; writing—review and editing, T.W.; visualization, B.K.; supervision, T.W. All authors have read and agreed to the published version of the manuscript.

Funding

This research received no external funding.

Data Availability Statement

Not applicable.

Acknowledgments

The authors acknowledge the financial support for excellent technological teams from the Faculty of Chemical Technology, University of Pardubice.

Conflicts of Interest

The authors declare no conflict of interest.

References

  1. Varjani, S.; Rakholiya, P.; Shindhal, T.; Shah, A.V.; Ngo, H.H. Trends in dye industry effluent treatment and recovery of valueadded products. J. Water Process Eng. 2021, 39, 101734. [Google Scholar] [CrossRef]
  2. Sen, S.K.; Raut, S.; Bandyopadhyay, P.; Raut, S. Fungal decolouration and degradation of azo dyes: A review. Fungal Biol. Rev. 2016, 30, 112–133. [Google Scholar] [CrossRef]
  3. Selvaraj, V.; Karthika, T.S.; Mansiya, C.; Alagar, M. An over review on recently developed techniques, mechanisms and intermediate involved in the advanced azo dye degradation for industrial applications. J. Mol. Struct. 2021, 1224, 129195. [Google Scholar] [CrossRef]
  4. Gong, R.; Li, M.; Yang, C.; Sun, Y.; Chen, J. Removal of cationic dyes from aqueous solution by adsorption on peanut hull. J. Hazard. Mater. 2005, 121, 247–250. [Google Scholar] [CrossRef]
  5. Cai, Y.; David, S.; Pailthorpe, M. Dyeing of jute and jute/cotton blend fabrics with 2:1 pre-metallised dyes. Dye. Pigment. 2000, 45, 161–168. [Google Scholar] [CrossRef]
  6. Ding, Y.; Freeman, H.S. Mordant dye application on cotton: Optimisation and combination with natural dyes. Color. Technol. 2017, 133, 369–375. [Google Scholar] [CrossRef]
  7. Sheikh, M.; Karim, R.; Farouqui, A.N.; Yahya, R.; Hassan, A. Effect of Acid Modification on Dyeing Properties of Rajshahi Silk Fabric with Different Dye Classes. Fibers Polym. 2011, 12, 642–647. [Google Scholar] [CrossRef]
  8. Sheikh, R.K.; Faruqui, A.N. A Comparative Study on Dyeing Behavior of Modified Rajshahi Silk Fabric with Reactive Orange 14, Direct Yellow 29 and Mordant Blue 9 Dyes. Man-Made Text. India 2010, 53, 10. [Google Scholar]
  9. Edwards, L.C.; Freeman, H.S. Synthetic dyes based on environmental considerations. Part 3: Aquatic toxicity of iron-complexed azo dyes. Color. Technol. 2005, 121, 265–270. [Google Scholar] [CrossRef]
  10. Gao, H.W.; Lin, J.; Li, W.Y.; Hu, Z.J.; Zhang, Y.L. Formation of shaped barium sulfate-dye hybrids: Waste dye utilization for eco-friendly treatment of wastewater. Environ. Sci. Pollut. Res. 2010, 17, 78–83. [Google Scholar] [CrossRef]
  11. Angelakis, A.; Snyder, S. Wastewater treatment and reuse: Past, present, and future. Water 2015, 7, 4887–4895. [Google Scholar] [CrossRef] [Green Version]
  12. Ran, J.H.; Shushina, I.; Priazhnikova, V.; Telegin, F. Inhibition of Mordant Dyes Destruction in Fenton Reaction. Adv. Mater. Res. 2013, 821, 493–496. [Google Scholar] [CrossRef]
  13. Šimek, M.; Mikulášek, P.; Kalenda, P.; Weidlich, T. Possibilities for removal of chlorinated dye Mordant Blue 9 from model wastewater. Chem. Pap. 2016, 70, 470–476. [Google Scholar] [CrossRef]
  14. Mishra, G.; Tripathy, M. A critical review of the treatments for decolourization of textile effluent. Colourage 1993, 40, 35–38. [Google Scholar]
  15. Xavier, S.; Gandhimathi, R.; Nidheesh, P.V.; Ramesh, S.T. Comparison of homogeneous and heterogeneous Fenton processes for the removal of reactive dye Magenta MB from aqueous solution. Desalin. Water Treat. 2015, 53, 109–118. [Google Scholar] [CrossRef]
  16. Nidheesh, P.V.; Gandhimathi, R.; Ramesh, S.T. Degradation of dyes from aqueous solution by Fenton processes: A review. Environ. Sci. Pollut. Res. 2013, 20, 2099–2132. [Google Scholar] [CrossRef]
  17. Nidheesh, P.V.; Gandhimathi, R. Trends in electro-Fenton process for water and wastewater treatment: An overview. Desalination 2012, 299, 1–15. [Google Scholar] [CrossRef]
  18. Pervez, M.N.; Telegin, F.Y.; Cai, Y.; Xia, D.; Zarra, T.; Naddeo, V. Efficient Degradation of Mordant Blue 9 Using the Fenton-Activated Persulfate System. Water 2019, 11, 2532. [Google Scholar] [CrossRef] [Green Version]
  19. Gulkaya, I.; Surucu, G.A.; Dilek, F.B. Importance of H2O2/Fe2+ ratio in Fenton’s treatment of a carpet dyeing wastewater. J. Hazard. Mater. 2006, 136, 763–769. [Google Scholar] [CrossRef]
  20. Olmez-Hanci, T.; Arslan-Alaton, I. Comparison of sulfate and hydroxyl radical based advanced oxidation of phenol. Chem. Eng. J. 2013, 224, 10–16. [Google Scholar] [CrossRef]
  21. Rastogi, A.; Al-Abed, S.R.; Dionysiou, D.D. Sulfate radical-based ferrous–peroxymonosulfate oxidative system for PCBs degradation in aqueous and sediment systems. Appl. Catal. B Environ. 2009, 85, 171–179. [Google Scholar] [CrossRef]
  22. Rao, Y.; Qu, L.; Yang, H.; Chu, W. Degradation of carbamazepine by Fe (II)-activated persulfate process. J. Hazard. Mater. 2014, 268, 23–32. [Google Scholar] [CrossRef]
  23. Wang, S.; Wu, J.; Lu, X.; Xu, W.; Gong, Q.; Ding, J.; Dan, B.; Xie, P. Removal of acetaminophen in the Fe2+/persulfate system: Kinetic model and degradation pathways. Chem. Eng. J. 2019, 358, 1091–1100. [Google Scholar] [CrossRef]
  24. Shang, W.; Dong, Z.; Li, M.; Song, X.; Zhang, M.; Jiang, C.; Feiyun, S. Degradation of diatrizoate in water by Fe (II)-activated persulfate oxidation. Chem. Eng. J. 2019, 361, 1333–1344. [Google Scholar] [CrossRef]
  25. Zhu, J.-P.; Lin, Y.-L.; Zhang, T.-Y.; Cao, T.-C.; Xu, B.; Pan, Y.; Zhang, X.-T.; Gao, N.-Y. Modelling of iohexol degradation in a Fe (II)-activated persulfate system. Chem. Eng. J. 2019, 367, 86–93. [Google Scholar] [CrossRef]
  26. Kusic, H.; Peternel, I.; Ukic, S.; Koprivanac, N.; Bolanca, T.; Papic, S.; Bozic, A.L. Modeling of iron activated persulfate oxidation treating reactive azo dye in water matrix. Chem. Eng. J. 2011, 172, 109–121. [Google Scholar] [CrossRef]
  27. Rodriguez, S.; Vasquez, L.; Costa, D.; Romero, A.; Santos, A. Oxidation of Orange G by persulfate activated by Fe (II), Fe (III) and zero valent iron (ZVI). Chemosphere 2014, 101, 86–92. [Google Scholar] [CrossRef]
  28. Made in China, Persulphate Price. Available online: https://www.made-in-china.com/products-search/hot-china-products/Persulphate_Price.html#:~:text=Sodium%20Persulfate%20Na2s2o8%20Factory%20Supply%20Plant%207775-27-1,PriceSodium%20Persulphate%20FOB%20Price%3A%20US%20%24%20900-1160%2F%20T (accessed on 11 November 2022).
  29. Procurement Resource, Hydrogen Peroxide Price Trends. Available online: https://www.procurementresource.com/resource-center/hydrogen-peroxide-price-trends (accessed on 11 November 2022).
  30. Weidlich, T.; Kamenická, B.; Melánová, K.; Čičmancová, V.; Komersová, A.; Čermák, J. Hydrodechlorination of different chloroaromatic compounds at room temperature and ambient pressure—Differences in reactivity of Cu-and Ni-Based Al alloys in an alkaline aqueous solution. Catalysts 2021, 10, 994. [Google Scholar] [CrossRef]
  31. Bendová, H.; Kamenická, B.; Weidlich, T.; Beneš, L.; Vlček, M.; Lacina, P.; Švec, P. Application of Raney Al-Ni alloy for simple hydrodehalogenation of Diclofenac and other halogenated biocidal contaminants in alkaline aqueous solution under ambient conditions. Materials 2022, 15, 3939. [Google Scholar] [CrossRef]
  32. Lin, Y.T.; Weng, C.H.; Chen, F.Y. Effective removal of AB24 dye by nano/micro-size zero-valent iron. Sep. Purif. Technol. 2008, 64, 26–30. [Google Scholar] [CrossRef]
  33. Raman, C.D.; Kanmani, S. Textile dye degradation using nano zero valent iron: A review. J. Environ. Manag. 2016, 177, 341–355. [Google Scholar] [CrossRef]
  34. Fan, J.; Guo, Y.; Wang, J.; Fan, M. Rapid decolorization of azo dye methyl orange in aqueous solution by nanoscale zerovalent iron particles. J. Hazard. Mater. 2009, 166, 904–910. [Google Scholar] [CrossRef]
  35. Nidheesh, P.V.; Khatri, J.; Singh, T.A.; Gandhimathi, R.; Ramesh, S.T. Review of zero-valent aluminium based water and wastewater treatment methods. Chemosphere 2018, 200, 621–631. [Google Scholar] [CrossRef]
  36. Yang, B.; Zhang, F.; Deng, S.; Yu, G.; Zhang, H.; Xiao, J.; Shen, J. A facile method for the highly efficient hydrodechlorination of 2-chlorophenol using Al-Ni alloy in the presence of fluorine ion. J. Chem. Eng. 2012, 209, 79–85. [Google Scholar] [CrossRef]
  37. Reife, A.; Freeman, H.S. Environmental Chemistry of Dyes and Pigments, 1st ed.; John Wiley & Sons:: Hoboken, NJ, USA, 1996; p. 352. ISBN 978-0-471-58927-3. [Google Scholar]
  38. Martins, A.; Nelson, N. Adsorption of a textile dye on commercial activated carbon: A simple experiment to explore the role of surface chemistry and ionic strength. J. Chem. Educ. 2015, 92, 143–147. [Google Scholar] [CrossRef]
  39. Tomic, N.M.; Dohcevic-Mitrovic, Z.D.; Paunović, N.M.; Mijin, D.Z.; Radić, N.D.; Grbic, B.V.; Bajuk-Bogdanovic, D.V. Nanocrystalline CeO2 δ as effective adsorbent of azo dyes. Langmuir 2014, 30, 11582–11590. [Google Scholar] [CrossRef] [Green Version]
  40. Kumar, M.; Venugopal, A.K.P.; Pakshirajan, K. Novel biologically synthesized metal nanopowder from wastewater for dye removal application. Environ. Sci. Pollut. Res. 2022, 29, 38478–38492. [Google Scholar] [CrossRef]
  41. Singh, S.; Pakshirajan, K.; Daverey, A. Screening and optimization of media constituents for decolourization of Mordant Blue-9 dye by Phanerochaete chrysosporium. Clean Technol. Environ. Policy 2010, 12, 313–323. [Google Scholar] [CrossRef]
  42. Yassen, D.A.; Scholz, M. Textile dye wastewater characteristics and constituents of synthetic effluents: A critical review. Int. J. Environ. Sci. Technol. 2019, 16, 1193–1226. [Google Scholar] [CrossRef] [Green Version]
  43. Kremer, M.L. The Fenton reaction. Dependence of the rate on pH. J. Phys. Chem. A. 2003, 107, 1734–1741. [Google Scholar] [CrossRef]
  44. Igbinosa, E.O.; Odjadjare, E.E.; Chigor, V.N.; Igbinosa, I.H.; Emoghene, A.O.; Ekhaise, F.O.; Igiehon, N.O.; Idemudia, O.G. Toxicological profile of chlorophenols and their derivatives in the environment: The public health perspective. Sci. World J. 2013, 11, 460215. [Google Scholar] [CrossRef] [Green Version]
  45. Weidlich, T.; Prokes, L.; Pospisilova, D. Debromination of 2,4,6-tribromophenol coupled with biodegradation. Cent. Eur. J. Chem. 2013, 11, 979. [Google Scholar] [CrossRef]
  46. Bousalah, D.; Zazoua, H.; Boudjemaa, A.; Benmounah, A.; Bachari, K. Degradation of Indigotine food dye by Fenton and photo-Fenton processes. Int. J. Environ. Anal. Chem. 2020, 102, 4609. [Google Scholar] [CrossRef]
  47. Kang, S.F.; Liao, C.H.; Chen, M.C. Pre-oxidation and coagulation of textile wastewater by the Fenton process. Chemosphere 2002, 46, 923–928. [Google Scholar] [CrossRef]
  48. Zhang, W.X. Nanoscale iron particles for environmental remediation: An overview. J. Nanoparticle Res. 2003, 5, 323–332. [Google Scholar] [CrossRef]
  49. Weidlich, T.; Kamenicka, B. Recycling of Spent Hydrodehalogenation Catalysts–Problems Dealing with Separation of Aluminium. Inz. Miner. 2019, 21, 177–182. [Google Scholar] [CrossRef]
  50. Weidlich, T.; Krejcova, A.; Prokes, L. Hydrodebromination of 2,4,6-tribromophenol in aqueous solution using Devarda’s alloy. Monatsh. Chem. 2013, 144, 155–162. [Google Scholar] [CrossRef]
  51. Bendova, H.; Weidlich, T. Application of diffusion dialysis in hydrometallurgical separation of nickel from spent Raney Ni catalyst. Sep. Sci. Technol. 2018, 53, 1218–1222. [Google Scholar] [CrossRef]
  52. Weidlich, T.; Oprsal, J.; Krejcova, A.; Jasurek, B. Effect of glucose on lowering Al-Ni alloy consumption in dehalogenation of halogenoanilines. Monatsh. Chem. 2015, 146, 613–620. [Google Scholar] [CrossRef]
  53. Made in China. H2SO4 Price. Available online: https://kunyabiological.en.made-in-china.com/product/kZMtfiCTMFWw/China-Sulfuric-Acid-with-Competitive-Price-and-CAS-No-7664-93-9.html (accessed on 23 January 2023).
  54. Sigma Aldrich. H2O2 Price. Available online: https://www.sigmaaldrich.com/CZ/en/substance/hydrogenperoxide34017722841 (accessed on 23 January 2023).
  55. Sigma Aldrich. FeSO4 Price. Available online: https://www.sigmaaldrich.com/CZ/en/substance/ironiisulfateheptahydrate278017782630 (accessed on 23 January 2023).
  56. AliExpress. Fe0 Price. Available online: https://www.aliexpress.com/item/1005003952039242.html?spm=a2g0o.productlist.main.1.666b1ebeXVNzaz&algo_pvid=567a960c-734e-414b-979d-f5ea646666da&algo_exp_id=567a960c-734e-414b-979d-f5ea646666da-0&pdp_ext_f=%7B%22sku_id%22%3A%2212000030178526057%22%7D&pdp_npi=2%40dis%21CZK%21367.31%21367.31%21%21%21%21%21%40214528be16744809367621410d06b6%2112000030178526057%21sea&curPageLogUid=hPMiO1R1R4b7 (accessed on 23 January 2023).
  57. Amazon. Al0 Price. Available online: https://www.amazon.com/Aluminum-Powder-Pound-MS-MetalShipper/dp/B0849WHSTY/ref=sr_1_1?crid=32BXCVP7ZHZH1&keywords=aluminum+powder&qid=1674482314&sprefix=%2Caps%2C1251&sr=8-1 (accessed on 23 January 2023).
  58. Made in China. NaOH Price. Available online: https://highmountainchem.en.made-in-china.com/product/HElUSyYxsrhD/China-Sodium-Hydroxide-Caustic-Soda-Flakes-Alkali-99-Naoh-CAS-1310-73-2.html (accessed on 23 January 2023).
  59. AliExpress. Ni0 Price. Available online: https://www.aliexpress.com/item/1005004187537341.html?spm=a2g0o.productlist.main.1.6f4ePBR5PBR5j9&algo_pvid=bab4e3ef-19f2-475e-b186-02000b20af84&algo_exp_id=bab4e3ef-19f2-475e-b186-02000b20af84-0&pdp_ext_f=%7B%22sku_id%22%3A%2212000028321382122%22%7D&pdp_npi=2%40dis%21CZK%21457.29%21251.53%21%21%21%21%21%402145288516744811272258567d0761%2112000028321382122%21sea&curPageLogUid=sc5TkfWdj7Qm (accessed on 23 January 2023).
  60. Fisher Scientific. Al-Ni Alloy Price. Available online: https://www.fishersci.fi/shop/products/aluminum-nickel-raney-type-alloy-powder-al-ni-50-50-thermo-scientific/11946951 (accessed on 23 January 2023).
  61. SRL CHEM. NaBH4 Price. Available online: https://srlchem.com/products/product_details/productId/1132 (accessed on 23 January 2023).
  62. India Global Mart. Na2S2O5 Price. Available online: https://dir.indiamart.com/impcat/sodium-metabisulfite.html (accessed on 23 January 2023).
Figure 1. The chemical structure of anionic azo dye Mordant Blue 9.
Figure 1. The chemical structure of anionic azo dye Mordant Blue 9.
Catalysts 13 00460 g001
Figure 2. Results of the oxidative degradation of MB9 using an excess of H2O2. (Appropriate quantity of H2O2 was added to 0.05 mmol of MB9 dissolved in 200 mL of H2O, with a reaction time of 20 h).
Figure 2. Results of the oxidative degradation of MB9 using an excess of H2O2. (Appropriate quantity of H2O2 was added to 0.05 mmol of MB9 dissolved in 200 mL of H2O, with a reaction time of 20 h).
Catalysts 13 00460 g002
Figure 3. A comparison of the effect of adding FeSO4 to the mixture of H2O2 and MB9 on COD and MB9 removal efficiency. (H2O2 and subsequently FeSO4 were added to 0.05 mmol of MB9 dissolved in 200 mL of H2O).
Figure 3. A comparison of the effect of adding FeSO4 to the mixture of H2O2 and MB9 on COD and MB9 removal efficiency. (H2O2 and subsequently FeSO4 were added to 0.05 mmol of MB9 dissolved in 200 mL of H2O).
Catalysts 13 00460 g003
Figure 4. A comparison of MB9 oxidation using the Fenton reaction after 4 h of action. (H2O2 and subsequently FeSO4 were added to 0.05 mmol of MB9 dissolved in 200 mL of H2O).
Figure 4. A comparison of MB9 oxidation using the Fenton reaction after 4 h of action. (H2O2 and subsequently FeSO4 were added to 0.05 mmol of MB9 dissolved in 200 mL of H2O).
Catalysts 13 00460 g004
Figure 5. Summary of removal efficiencies obtained using different molar ratios between [Fe2+]/[H2O2]/[MB9]. (* H2O2 and subsequently FeSO4 were added to acidified 0.05 mmol of MB9 in 200 mL of H2O, with a reaction time of 20 h or 4 h).
Figure 5. Summary of removal efficiencies obtained using different molar ratios between [Fe2+]/[H2O2]/[MB9]. (* H2O2 and subsequently FeSO4 were added to acidified 0.05 mmol of MB9 in 200 mL of H2O, with a reaction time of 20 h or 4 h).
Catalysts 13 00460 g005
Figure 6. The effect of different FeSO4 and/or H2O2 dosages on the removal efficiencies. (H2O2 and subsequently FeSO4 were added to acidified 0.05 mmol of MB9 dissolved in 200 mL of H2O, with a reaction time of 20 h).
Figure 6. The effect of different FeSO4 and/or H2O2 dosages on the removal efficiencies. (H2O2 and subsequently FeSO4 were added to acidified 0.05 mmol of MB9 dissolved in 200 mL of H2O, with a reaction time of 20 h).
Catalysts 13 00460 g006
Figure 7. A comparison of the dependence of MB9 oxidative degradation on time under different dosages of H2O2 and FeSO4. (Appropriate quantities of H2O2 and FeSO4 were added to 0.05 mmol of MB9 dissolved in 200 mL of H2O).
Figure 7. A comparison of the dependence of MB9 oxidative degradation on time under different dosages of H2O2 and FeSO4. (Appropriate quantities of H2O2 and FeSO4 were added to 0.05 mmol of MB9 dissolved in 200 mL of H2O).
Catalysts 13 00460 g007
Figure 8. The reductive degradation of MB9 using ZVI. (ZVI was added to aqueous solution containing 0.05 mmol of MB9 in 100 mL of H2O acidified with 40 mmol of H2SO4, with a reaction time of 3 h).
Figure 8. The reductive degradation of MB9 using ZVI. (ZVI was added to aqueous solution containing 0.05 mmol of MB9 in 100 mL of H2O acidified with 40 mmol of H2SO4, with a reaction time of 3 h).
Catalysts 13 00460 g008
Figure 9. The reductive degradation of MB9 using different types of Al0 in an acidic environment. (Al0 was added to the solution of 0.05 mmol of MB9 and 40 mmol of H2SO4 in 100 mL of H2O, with a reaction time of 20 h) (n.d. = not determined).
Figure 9. The reductive degradation of MB9 using different types of Al0 in an acidic environment. (Al0 was added to the solution of 0.05 mmol of MB9 and 40 mmol of H2SO4 in 100 mL of H2O, with a reaction time of 20 h) (n.d. = not determined).
Catalysts 13 00460 g009
Figure 10. The reductive degradation of MB9 using different types of Al0 and their mixtures with nickel in an aqueous 50 mM NaOH solution. (Al0 and Ni0 were added to the solution of 0.05 mmol of MB9 and 5 mmol of NaOH in 100 mL of H2O, with a reaction time of 3 h).
Figure 10. The reductive degradation of MB9 using different types of Al0 and their mixtures with nickel in an aqueous 50 mM NaOH solution. (Al0 and Ni0 were added to the solution of 0.05 mmol of MB9 and 5 mmol of NaOH in 100 mL of H2O, with a reaction time of 3 h).
Catalysts 13 00460 g010
Figure 11. A comparison of rates of MB9 reductive degradation under different dosages of Al and NaOH or H2SO4. (Appropriate quantities of Al and NaOH/H2SO4 were added to 0.05 mmol of MB9 dissolved in 200 mL of H2O).
Figure 11. A comparison of rates of MB9 reductive degradation under different dosages of Al and NaOH or H2SO4. (Appropriate quantities of Al and NaOH/H2SO4 were added to 0.05 mmol of MB9 dissolved in 200 mL of H2O).
Catalysts 13 00460 g011
Figure 12. A comparison of AOX and MB9 removal caused by Raney Al-Ni alloy action. (Al-Ni alloy added to aqueous solutions of 0.05 mmol of MB9 and 5 mmol of NaOH in 100 mL of H2O, with a reaction time of 3 h).
Figure 12. A comparison of AOX and MB9 removal caused by Raney Al-Ni alloy action. (Al-Ni alloy added to aqueous solutions of 0.05 mmol of MB9 and 5 mmol of NaOH in 100 mL of H2O, with a reaction time of 3 h).
Catalysts 13 00460 g012
Scheme 1. Proposed reaction pathway for the reduction of MB9 accompanied by hydrodechlorination.
Scheme 1. Proposed reaction pathway for the reduction of MB9 accompanied by hydrodechlorination.
Catalysts 13 00460 sch001
Figure 13. A comparison of sorption abilities of tested Al-based reduction agents. (Mentioned quantities of metal(s) were added to the 0.05 mmol of MB9 dissolved in 100 mL of H2O, with a sorption time of 3 h).
Figure 13. A comparison of sorption abilities of tested Al-based reduction agents. (Mentioned quantities of metal(s) were added to the 0.05 mmol of MB9 dissolved in 100 mL of H2O, with a sorption time of 3 h).
Catalysts 13 00460 g013
Figure 14. A comparison of discoloration of MB9 using of 6 mmol of oxidant/reductant. (An appropriate quantity of reagents was added to 0.05 mmol of MB9 dissolved in 200 mL of H2O).
Figure 14. A comparison of discoloration of MB9 using of 6 mmol of oxidant/reductant. (An appropriate quantity of reagents was added to 0.05 mmol of MB9 dissolved in 200 mL of H2O).
Catalysts 13 00460 g014
Figure 15. Reductive removal of MB9 and AOX using reductant(s) based on NaBH4 action. (The above-mentioned reduction agents were added to the aq. solution of 0.1 mmol of MB9 in 200 mL of H2O, with a reaction time of 20 h).
Figure 15. Reductive removal of MB9 and AOX using reductant(s) based on NaBH4 action. (The above-mentioned reduction agents were added to the aq. solution of 0.1 mmol of MB9 in 200 mL of H2O, with a reaction time of 20 h).
Catalysts 13 00460 g015
Scheme 2. The proposed reaction scheme of MB9 reductive degradation using NaBH4/Na2S2O5.
Scheme 2. The proposed reaction scheme of MB9 reductive degradation using NaBH4/Na2S2O5.
Catalysts 13 00460 sch002
Figure 16. A comparison of the reaction rates of MB9 reductive degradation under different dosages of reductants. (An appropriate quantity of reagents was added to 0.05 mmol of MB9 dissolved in 200 mL of H2O).
Figure 16. A comparison of the reaction rates of MB9 reductive degradation under different dosages of reductants. (An appropriate quantity of reagents was added to 0.05 mmol of MB9 dissolved in 200 mL of H2O).
Catalysts 13 00460 g016
Figure 17. A comparison of reagent consumption and effectiveness of MB9 degradation. (An appropriate quantity of reagents was added to 0.05 mmol of MB9 dissolved in 200 mL of H2O, with a reaction time of # 3 h or * 20–21 h).
Figure 17. A comparison of reagent consumption and effectiveness of MB9 degradation. (An appropriate quantity of reagents was added to 0.05 mmol of MB9 dissolved in 200 mL of H2O, with a reaction time of # 3 h or * 20–21 h).
Catalysts 13 00460 g017
Table 1. A comparison of MB9 removal efficiencies caused by oxidation or reduction using different reactants at room temperature (calculated per mol of MB9).
Table 1. A comparison of MB9 removal efficiencies caused by oxidation or reduction using different reactants at room temperature (calculated per mol of MB9).
Applied Degradation MethodQuantity of Used Reagents per mol of MB9Efficiency of MB9
Discoloration
Other Removal Efficiencies
(%)
Ref.
Persulfate-based AOP at pH = 4.8816 mol of Na2S2O8
+ 14 mol of FeSO4
97%
(after 30 min)
60% of TOC
(after 30 min)
[18]
Fenton oxidation at
pH = 4.88
16 mol of H2O2
+ 14 mol of FeSO4
48% of MB9
(after 30 min)
38% of TOC
(after 30 min)
[18]
Fenton oxidation at
pH = 2–2.5
28 mol of H2SO4
120 mol of H2O2
+ 4 mol of FeSO4
86.1% of MB9
(after 3 h)
37.6% of COD
(after 3 h)
This work
Fenton oxidation at
pH = 2–2.5
28 mol of H2SO4
120 mol of H2O2
+ 4 mol of FeSO4
>99% of MB9
(after 20 h)
98.3% of AOX and 93.7% of COD
(after 20 h)
This work
Chemical reduction
ZVI
150 mol of Fe0
800 mol of H2SO4
99.5% of MB9
(after 3 h)
35.2% of AOX
(after 3 h)
This work
Chemical reduction
Al0 powder
370 mol of Al0
800 mol of H2SO4
97.5% of MB9
(after 20 h)
30.5% of AOX
(after 20 h)
This work
Chemical reduction
Al0 powder
200 mol of Al0
100 mol of NaOH
96.5% of MB9
(after 3 h)
41.4% of AOX
(after 3 h)
This work
Chemical reduction
Al0 powder
+ Ni0 powder
200 mol of Al0
50 mol of Ni0
100 mol of NaOH
96.7% of MB956.4% of AOX
(after 3 h)
This work
Chemical reduction
Raney Al-Ni
100 mol of Al0
used in Al-Ni
100 mol of NaOH
96.9% of MB9
(after 3 h)
94.5% of AOX
(after 3 h)
This work
Chemical reduction
Al0 powder
+ Raney Al-Ni
120 mol of Al0
480 mol of NaOH
44 mol of Al0 (in Al-Ni)
480 mol of NaOH
99% of MB9
(after 3 + 20 h)
91.7% of AOX
(after 3 + 20 h)
This work
Chemical reduction
NaBH4
132 mol of NaBH499.4% of MB9
(after 20 h)
68.7% of AOX
(after 20 h)
This work
Chemical reduction
NaBH4/Na2S2O5
66 mol of NaBH4
+ 66 mol of Na2S2O5
+ 18 mol of H2SO4
99.5% of MB9
(after 30 min)
95.9% of AOX
(after 20 h)
This work
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content.

Share and Cite

MDPI and ACS Style

Kamenická, B.; Weidlich, T. A Comparison of Different Reagents Applicable for Destroying Halogenated Anionic Textile Dye Mordant Blue 9 in Polluted Aqueous Streams. Catalysts 2023, 13, 460. https://doi.org/10.3390/catal13030460

AMA Style

Kamenická B, Weidlich T. A Comparison of Different Reagents Applicable for Destroying Halogenated Anionic Textile Dye Mordant Blue 9 in Polluted Aqueous Streams. Catalysts. 2023; 13(3):460. https://doi.org/10.3390/catal13030460

Chicago/Turabian Style

Kamenická, Barbora, and Tomáš Weidlich. 2023. "A Comparison of Different Reagents Applicable for Destroying Halogenated Anionic Textile Dye Mordant Blue 9 in Polluted Aqueous Streams" Catalysts 13, no. 3: 460. https://doi.org/10.3390/catal13030460

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.